Environmentally friendly tin stripping liquid and preparation method and application thereof

By adding a specific proportion of ionic liquid, surfactant and oxidant to the tin stripping liquid to form a protective film, the problem of nitric acid and hydrogen peroxide pollution in the existing tin stripping liquid is solved, and an environmentally friendly and corrosion-free tin removal effect is achieved. It is applicable In lead-free packaging, tin copper plating and tin bismuth plating improve peeling efficiency and safety.

CN118497759BActive Publication Date: 2024-11-22SUN SURFACE CHEM (SUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410661524.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-11-22
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

The existing tin stripping liquid contains a large amount of nitric acid and hydrogen peroxide, which leads to environmental pollution, difficulty in treating wastewater, high cost, and inability to effectively control hydrogen peroxide decomposition, affecting the effect of detinning.

Method used

Use an environmentally friendly tin stripping liquid without nitric acid, hydrofluoric acid, and hydrogen peroxide. By adding a specific proportion of ionic liquid, surfactant and oxidant to the tin stripping liquid, it forms a protective film to avoid corrosion of the substrate and improve peeling efficiency. And through a combination of specific organic acids and oxidants, the peeling effect and environmental protection are ensured.

Benefits of technology

It achieves an environmentally friendly and corrosion-free tin removal effect, avoids substrate pollution, pattern falling off or discoloration, and is suitable for lead-free packaging of tin copper plating and tin bismuth plating, improving peeling efficiency and safety and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of tin stripping liquid, and more specifically, to a preparation method and application of an environmentally friendly tin stripping liquid. The environmentally friendly tin stripping liquid, by mass percentage, comprises raw materials including: 20-30% organic acid, 1-3% oxidant, 1-3% ionic liquid, 1-2% surfactant, and water remainder. The present invention solves the problems that the existing tin stripping liquid contains a large amount of nitric acid, is not environmentally friendly, contains hydrogen peroxide, and cannot control the decomposition of hydrogen peroxide, resulting in poor effect and high cost. The tin stripping liquid provided by the present invention does not contain nitric acid, hydrofluoric acid, and hydrogen peroxide, is environmentally friendly, has a good tin removal effect, has no corrosive effect on the substrate, does not cause substrate pollution, does not cause pattern shedding or discoloration, and is particularly suitable for tin-copper plating and tin-bismuth plating of lead-free IC packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of tin stripping liquid, and more specifically, to a preparation method and application of an environmentally friendly tin stripping liquid. Background Art

[0002] IC packaging is an essential process to prevent the corrosion of chip circuits by impurities in the air and cause degradation of electrical performance, and to facilitate transportation. The packaging substrates used in the IC packaging process are usually etched to form different shapes. During the etching process, plating is usually used as a protective layer. At present, with the development of the lead-free trend, lead-free plating is mostly used, including pure tin plating or tin alloy plating, such as tin-copper plating and tin-bismuth plating. After the etching is completed, the plating needs to be removed for subsequent welding, assembly and reprocessing.

[0003] The tin stripping liquid used in the prior art is generally a nitric acid type tin stripping liquid, such as a Chinese patent with publication number CN106048612A, which discloses a method for removing a tin-containing layer on a substrate. The tin stripping liquid includes 5g / L-100g / L nitric acid, 70g / L-640g / L complexing agent, 10g / L-150g / L stabilizer, 0.5g / L-25g / L antioxidant, wherein the stabilizer includes at least one of a carboxylic acid compound, a urea compound, and an amino acid. Although the tin stripping liquid provided by the technical solution uses nitric acid with a relatively low content, NO2 is not generated, and pollution to the environment is reduced, but due to a large amount of nitric acid contained in the waste liquid, wastewater treatment is difficult.

[0004] A Chinese patent with publication number CN108468050A discloses a tin stripping solution and its application in tin stripping. Each liter of the tin stripping solution includes the following materials: 20-60ML of hydrogen peroxide, 300-700ML / L of methanesulfonic acid, 0-6g of benzotriazole per liter of the tin stripping solution, and the rest is water. This technical solution uses hydrogen peroxide as an oxidant, and methanesulfonic acid as an organic acid to provide a strong acid environment while having low corrosion to the substrate copper. Benzotriazole is added as a substrate copper protective agent to perform tin metal stripping, avoiding the large amount of alkali consumption in traditional methods, reducing waste discharge, and saving energy and protecting the environment. However, the decomposition rate of hydrogen peroxide is high. This technical solution requires the use of a specific hydrogen peroxide online analysis device and a hydrogen peroxide automatic addition device to control the hydrogen peroxide concentration, which is costly. Summary of the invention

[0005] The purpose of the present invention is to provide an environmentally friendly tin stripping liquid and a preparation method and application thereof, so as to solve the problems that the existing tin stripping liquid contains a large amount of nitric acid, is not environmentally friendly, contains hydrogen peroxide, and the decomposition of hydrogen peroxide cannot be controlled, resulting in poor effect and high cost. The tin stripping liquid provided by the present invention does not contain nitric acid, hydrofluoric acid, and hydrogen peroxide, is environmentally friendly, has a good tin removal effect, has no corrosive effect on the substrate, does not cause pollution to the substrate, and does not cause pattern shedding or discoloration. The tin stripping liquid is particularly suitable for tin-copper plating and tin-bismuth plating of lead-free IC packaging.

[0006] The first aspect of the present invention provides an environmentally friendly tin stripping liquid, wherein the raw materials include, by mass percentage: 20-30% organic acid, 1-3% oxidant, 1-3% ionic liquid, 1-2% surfactant, 0.5-1% complexing agent, and the balance water;

[0007] The ionic liquid is a mixture of 1-ethyl-3-methylimidazolium acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bis(trifluoromethanesulfonyl)imide; the mass ratio of the 1-ethyl-3-methylimidazolium acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bis(trifluoromethanesulfonyl)imide is 8-10:3-5:1-2.

[0008] The inventors found that adding ionic liquids to the tin stripping liquid system and acting together with surfactants can avoid the corrosion of the tin stripping liquid on the copper substrate. It is speculated that this is because the electrostatic attraction between the ionic liquid and the surfactant forms micelles, and a tight and uniform chemical adsorption protective film is formed on the surface of the substrate while stripping the tin and tin alloy coatings, thereby improving the corrosion inhibition of the substrate. At the same time, it was found that when the ionic liquid is a mixture of 1-ethyl-3-methylimidazolium acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bistrifluoromethanesulfonyl imide salt in a mass ratio of 8-10:3-5:1-2, the stripping efficiency of the tin stripping liquid is improved. The inventors speculate that this is because the compounded ionic liquid under this condition can improve the solubility of the organic acid and prevent the decomposition of the organic acid on the one hand, and on the other hand, the surface tension of the ionic liquid under this condition is low, and it can effectively penetrate into the tiny gaps of the coating, so that the organic acid is fully in contact with the tin and tin alloy coatings, thereby achieving a full reaction between the organic acid and tin, and improving the stripping efficiency of the tin and tin alloy coatings.

[0009] Preferably, the organic acid is selected from at least one of oxalic acid, citric acid, aminosulfonic acid, alkylsulfonic acid and formic acid.

[0010] Preferably, the organic acid is a mixture of oxalic acid, citric acid and alkyl sulfonic acid; the mass ratio of oxalic acid, citric acid and alkyl sulfonic acid is 5-7:3-5:3-5.

[0011] The inventors have found that by using oxalic acid, citric acid, and alkyl sulfonic acid in a mass ratio of 5-7:3-5:3-5 for compound use, tin and tin alloy coatings can be effectively stripped while avoiding contamination of the substrate. The inventors speculate that this is because the presence of the alkyl sulfonic acid can prevent the formation of tin citrate with low solubility due to the presence of citric acid through complexation, thereby avoiding contamination of the substrate.

[0012] Preferably, the number of carbon atoms in the alkyl sulfonic acid is 1-5, preferably methanesulfonic acid.

[0013] Preferably, the oxidant is selected from at least one of potassium permanganate, sodium permanganate, ferric chloride, ferric nitrate and cerium oxide.

[0014] Preferably, the oxidant is a mixture of ferric chloride, cerium oxide and potassium permanganate; the mass ratio of the ferric chloride, cerium oxide and potassium permanganate is 3-5:1:2-3.

[0015] The inventors found that when the oxidant is a mixture of ferric chloride, cerium oxide and potassium permanganate, corrosion and pollution of the substrate can be avoided while improving the stripping effect of the tin stripping solution. The inventors speculate that the oxidant at this mass ratio can improve the reaction activity of organic acid with tin and tin alloy coatings, making it easier for the organic acid to form a complex with tin while cerium oxide can coordinate with a surfactant to form a coordination compound with a larger molecular weight, forming a dense protective film on the substrate surface to avoid corrosion of the substrate, and in addition, the presence of ferric chloride can also inhibit the generation of metastannic acid, while further improving the stripping effect of the tin stripping solution, avoiding pollution of the substrate surface.

[0016] Preferably, the surfactant is selected from at least one of alkylphenol polyoxyethylene ether, cardanol polyoxyethylene ether, fatty alcohol polyoxyethylene ether, fatty acid polyoxyethylene ether, and fatty acid ester polyoxyethylene ether.

[0017] Preferably, the surfactant is a mixture of cardanol polyoxyethylene ether and fatty alcohol polyoxyethylene ether.

[0018] Preferably, the mass ratio of the cardanol polyoxyethylene ether to the fatty alcohol polyoxyethylene ether is 4-6:2-4.

[0019] Preferably, the fatty alcohol polyoxyethylene ether is C 16 -C 18 Alcohol polyoxyethylene ether.

[0020] The specific organic acid and oxidant used in the present invention can improve the stripping effect of the tin stripping solution while avoiding corrosion and pollution of the substrate. However, the added cerium oxide has poor dispersibility, which limits its use in the tin stripping solution. The inventors found that when the surfactant is a mixture of cardanol polyoxyethylene ether and fatty alcohol polyoxyethylene ether in a mass ratio of 4-6:2-4, the fatty alcohol polyoxyethylene ether is C 16 -C 18 When alcohol polyoxyethylene ether is added, the dispersibility of cerium oxide can be improved. At the same time, it is unexpectedly found that the etching pattern can be prevented from falling off or discoloring. The inventors speculate that this is because the surfactant under this condition can reduce the surface tension of the system and form micelles, which is beneficial to the dispersion of cerium oxide. 16 -C 18 Alcohol polyoxyethylene ether has a different migration speed than cardanol polyoxyethylene ether, and can form a multi-layer protective film on the surface of the etching pattern, thereby preventing the susceptible etching pattern from falling off or discoloring.

[0021] Preferably, the complexing agent is selected from at least one of sodium benzoate, sodium ethylenediaminetetramethylenephosphate, and potassium sodium tartrate, preferably sodium benzoate.

[0022] A second aspect of the present invention provides a method for preparing an environmentally friendly tin stripping solution, comprising the following steps:

[0023] S1. Add ionic liquid into water and stir until dissolved;

[0024] S2. Add organic acid, oxidant and complexing agent into S1 solution, then add surfactant and stir evenly.

[0025] A third aspect of the present invention provides an application of an environmentally friendly tin stripping liquid in IC packaging.

[0026] Beneficial effects:

[0027] 1. The present invention adds ionic liquid to the tin stripping liquid system, which works together with the surfactant to avoid the corrosion of the tin stripping liquid on the copper substrate. When the ionic liquid is a mixture of 1-ethyl-3-methylimidazole acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bistrifluoromethanesulfonimide salt in a mass ratio of 8-10:3-5:1-2, the stripping efficiency of the tin stripping liquid is improved.

[0028] 2. The present invention uses oxalic acid, citric acid and alkyl sulfonic acid in a mass ratio of 5-7:3-5:3-5 for compound use, which can effectively strip off the tin and tin alloy coatings while avoiding contamination of the substrate.

[0029] 3. When the oxidant of the present invention is a mixture of ferric chloride, cerium oxide and potassium permanganate, the stripping effect of the tin stripping solution can be improved while corrosion and pollution of the substrate can be avoided.

[0030] 4. In the present invention, when the surfactant is a mixture of cardanol polyoxyethylene ether and fatty alcohol polyoxyethylene ether in a mass ratio of 4-6:2-4, the fatty alcohol polyoxyethylene ether is C 16 -C 18 When alcohol polyoxyethylene ether is added, the solubility of cerium oxide can be improved. At the same time, it is unexpectedly found that the etching pattern can be prevented from falling off or discoloring. DETAILED DESCRIPTION

[0031] In order to better explain the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the examples in the embodiments of the present invention. The embodiments described are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other implementation methods obtained by those skilled in the art without making creative work are within the scope of protection of the present invention. The experimental methods in the following embodiments, unless otherwise specified, are conventional methods, and the materials, reagents, etc. used in the following embodiments, unless otherwise specified, can be obtained from commercial channels.

[0032] Example 1

[0033] Example 1 provides an environmentally friendly tin stripping liquid, wherein the raw materials include, by mass percentage: 25% organic acid, 1% oxidant, 2% ionic liquid, 1.1% surfactant, 0.9% complexing agent, and the balance water;

[0034] The ionic liquid is a mixture of 1-ethyl-3-methylimidazolium acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bis(trifluoromethanesulfonyl)imide; the mass ratio of the 1-ethyl-3-methylimidazolium acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bis(trifluoromethanesulfonyl)imide is 9:4:1.

[0035] Among them, 1-ethyl-3-methylimidazole acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bis(trifluoromethanesulfonyl)imide salt were all purchased from Zhejiang Lande Energy Technology Development Co., Ltd.

[0036] The organic acid is a mixture of oxalic acid, citric acid and methanesulfonic acid; the mass ratio of the oxalic acid, citric acid and methanesulfonic acid is 6:4:4.

[0037] The oxidant is a mixture of ferric chloride, cerium oxide and potassium permanganate; the mass ratio of the ferric chloride, cerium oxide and potassium permanganate is 4:1:2.

[0038] The surfactant is a mixture of cardanol polyoxyethylene ether and fatty alcohol polyoxyethylene ether.

[0039] The mass ratio of the cardanol polyoxyethylene ether to the fatty alcohol polyoxyethylene ether is 5:3.

[0040] Among them, cardanol polyoxyethylene was purchased from Shanghai Bangao Chemical Co., Ltd., model: BGF-6.

[0041] The fatty alcohol polyoxyethylene ether is C16-C18 alcohol polyoxyethylene ether, purchased from Shanghai Bangao Chemical Co., Ltd., model: O-9.

[0042] The complexing agent is sodium benzoate.

[0043] A method for preparing an environmentally friendly tin stripping solution comprises the following steps:

[0044] S1. Add ionic liquid into water and stir until dissolved;

[0045] S2. Add organic acid, oxidant and complexing agent into S1 solution, then add surfactant and stir evenly.

[0046] Application of an environmentally friendly tin stripping liquid in IC packaging.

[0047] Example 2

[0048] Example 2 provides an environmentally friendly tin stripping liquid, a preparation method and application thereof. Its specific implementation method is the same as that of Example 1, except that, by mass percentage, the raw materials include: 20% organic acid, 1% oxidant, 1.4% ionic liquid, 1% surfactant, 0.6% complexing agent, and the remainder water.

[0049] Example 3

[0050] Example 3 provides an environmentally friendly tin stripping liquid, a preparation method and application thereof. Its specific implementation method is the same as that of Example 1, except that, by mass percentage, the raw materials include: 30% organic acid, 2% oxidant, 2% ionic liquid, 2% surfactant, 1% complexing agent, and the remainder water.

[0051] Comparative Example 1

[0052] Comparative Example 1 provides an environmentally friendly tin stripping liquid, a preparation method and an application thereof. Its specific implementation method is the same as that of Example 1, except that the mass ratio of the 1-ethyl-3-methylimidazole acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bistrifluoromethanesulfonimide salt is 7:6:1.

[0053] Comparative Example 2

[0054] Comparative Example 2 provides an environmentally friendly tin stripping liquid, a preparation method and an application thereof. Its specific implementation method is the same as Example 1, except that 1-ethyl-3-methylimidazole acetate is replaced by 1-ethylpyridine tetrafluoroborate, and 1-ethylpyridine tetrafluoroborate is purchased from Zhejiang Lande Energy Technology Development Co., Ltd.

[0055] Comparative Example 3

[0056] Comparative Example 3 provides an environmentally friendly tin stripping liquid, a preparation method and application thereof. The specific implementation method is the same as that of Example 1, except that the organic acid is oxalic acid and citric acid; the mass ratio of oxalic acid to citric acid is 6:4.

[0057] Comparative Example 4

[0058] Comparative Example 4 provides an environmentally friendly tin stripping liquid, a preparation method and application thereof, and its specific implementation method is the same as that of Example 1, except that the mass ratio of the oxalic acid, citric acid and methanesulfonic acid is 4:2:6.

[0059] Comparative Example 5

[0060] Comparative Example 5 provides an environmentally friendly tin stripping liquid, a preparation method and an application thereof. Its specific implementation method is the same as that of Example 1, except that the oxidant is a mixture of ferric chloride and potassium permanganate; the mass ratio of ferric chloride to potassium permanganate is 4:2.

[0061] Comparative Example 6

[0062] Comparative Example 6 provides an environmentally friendly tin stripping liquid, a preparation method and application thereof. Its specific implementation method is the same as Example 1, except that the fatty alcohol polyoxyethylene ether is replaced by octylphenol polyoxyethylene ether, which is purchased from Shanghai Bangao Chemical Co., Ltd., model: O-9.

[0063] Comparative Example 7

[0064] Comparative Example 7 provides an environmentally friendly tin stripping solution and a preparation method and application thereof. The specific implementation method is the same as that of Example 1, except that C 16 -C 18 Alcohol polyoxyethylene ether is C2-C 14 Alcohol polyoxyethylene ether was purchased from Shanghai Bangao Chemical Co., Ltd., model: A110.

[0065] Performance test: The environmentally friendly tin stripping liquids of Examples 1-3 and Comparative Examples 1-7 were tested as follows:

[0066] (1) Stripping rate: A pure tin plate of size 1 cm × 1 cm was completely immersed in an environmentally friendly tin stripping solution. After standing at 25°C for 15 seconds, the tin plate was taken out and dried. The weight difference before and after the weight difference was measured.

[0067] Stripping rate (μm / min) = (weight of tin plate before treatment (g) - weight of tin plate after treatment (g)) ÷ area of ​​tin plate (m 2 )÷7.28(g / cm 3 )÷processing time (min); the density of tin plate is 7.28g / cm 3 .

[0068] (2) Substrate corrosion performance: A pure copper plate of 1 cm × 1 cm in size was completely immersed in an environmentally friendly tin stripping solution. After standing for 15 seconds at 25°C, the copper plate was taken out and dried. The mass difference before and after weighing the copper plate was measured.

[0069] Corrosion rate (μm / min) = (weight of copper plate before treatment (g) - weight of copper plate after treatment (g)) ÷ area of ​​copper plate (m 2 )÷8.92(g / cm 3 )÷processing time (min); the density of the copper plate is 8.92g / cm 3 .

[0070] (3) Whether the substrate is contaminated: Immerse the IC substrate completely in environmentally friendly tin stripping liquid, let it stand at 25°C for 15 seconds, then take out the IC substrate and dry it. Visually observe whether there are impurities on the copper surface and whether it is shiny.

[0071] (4) Whether the pattern falls off or changes color: Immerse the IC substrate completely in environmentally friendly tin stripping liquid. After standing for 15 seconds at 25°C, take out the IC substrate and dry it. Observe whether the pattern falls off or changes color.

[0072] The test results are shown in Table 1:

[0073] Table 1 Performance test

[0074]

[0075] It can be seen from Table 1 that due to the change in the ionic liquid conditions, the stripping rates of the tin stripping solutions obtained in Comparative Examples 1 and 2 are reduced compared to those obtained in Example 1, while the corrosion rates are increased.

[0076] Due to the change in organic acid conditions, the stripping rate of the tin stripping solution obtained in Comparative Example 3-4 is lower than that in Example 1, a small amount of white impurities appear, and the copper surface is not bright.

[0077] In Comparative Example 5, due to the change in oxidant conditions, the stripping rate of the tin stripping solution obtained in Example 1 is reduced while the corrosion rate is increased.

[0078] In Comparative Examples 6-7, due to the change in surfactant conditions, the stripping rate of the tin stripping solution obtained in Example 1 was reduced while the corrosion rate was increased, and the pattern fell off or changed color.

[0079] The above description is only a specific embodiment of the present invention, and does not limit the patent scope of the present invention. Any equivalent transformation made by the present invention, or directly or indirectly applied in other related technical fields, is also included in the patent protection scope of the present invention.

Claims

1. An environmentally friendly tin stripping solution, It is characterized in that The raw materials include, by mass percentage: 20-30% organic acid, 1-3% oxidant, 1-3% ionic liquid, 1-2% surfactant, 0.5-1% complexing agent, and the balance water; The organic acid is a mixture of oxalic acid, citric acid and alkyl sulfonic acid; the mass ratio of oxalic acid, citric acid and alkyl sulfonic acid is 5-7:3-5:3-5; The oxidant is a mixture of ferric chloride, cerium oxide and potassium permanganate; the mass ratio of ferric chloride, cerium oxide and potassium permanganate is 3-5:1:2-3; The ionic liquid is a mixture of 1-ethyl-3-methylimidazolium acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bis(trifluoromethanesulfonyl)imide; the mass ratio of the 1-ethyl-3-methylimidazolium acetate, N-methyl-N-butylpiperidinium tetrafluoroborate, and tributylmethylammonium bis(trifluoromethanesulfonyl)imide is 8-10:3-5:1-2; The surfactant is a mixture of cardanol polyoxyethylene ether and fatty alcohol polyoxyethylene ether; the mass ratio of the cardanol polyoxyethylene ether to the fatty alcohol polyoxyethylene ether is 4-6:2-4; The fatty alcohol polyoxyethylene ether is C 16 -C 18 Alcohol polyoxyethylene ether.

2. A method for preparing an environmentally friendly tin stripping solution according to claim 1, It is characterized in that The following steps are involved: S1. Add ionic liquid into water and stir until dissolved; S2. Add organic acid, oxidant and complexing agent into S1 solution, then add surfactant and stir evenly.

3. Application of the environmentally friendly tin stripping liquid according to claim 1 in IC packaging.