Preparation method and application of a polysulfide polymer intercalated nickel-molybdenum double hydroxide composite material
By using needle-like NiMo double transition metal hydroxide prepared by hydrothermal method in the electrocatalyst and performing polysulfide polymer intercalation treatment to form a nickel-molybdenum double metal hydroxide composite material, the problem of slow kinetics of the electrocatalyst is solved , achieving excellent electrocatalytic oxygen evolution performance and stability, replacing the application of precious metal catalysts.
Patent Information
- Application Number
- CN202410958844.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Existing electrocatalysts have the problem of slow kinetics in water splitting. In particular, the oxygen evolution reaction (OER) at the anode needs to overcome a huge activation energy barrier. Moreover, noble metal catalysts such as Pt-based and Ir-based catalysts are expensive and scarce and cannot be used on a large scale. Large-scale commercial applications.
The needle-shaped NiMo double transition metal hydroxide is prepared by hydrothermal method, and the polysulfide polymer is intercalated onto it by the inverse sulfide method to form a polysulfide polymer intercalated nickel molybdenum double metal hydroxide composite material. As an electrocatalyst, nanoneedle structures and polysulfide polymer vulcanization are utilized to increase specific surface area and electron transport capabilities.
It achieves excellent electrocatalytic oxygen evolution performance under alkaline conditions, reduces overpotential, increases the number of electrocatalytic active sites, and the material is stable, avoiding accidental aggregation during the electrochemical process, and enhancing the electron donor capability .
Smart Images

Figure CN118497826B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrocatalytic water decomposition, and specifically relates to a preparation method and application of a polysulfide polymer intercalated nickel-molybdenum double metal hydroxide composite material. Background Art
[0002] Electrocatalytic water splitting technology is a technology that uses electrochemical methods to decompose water into hydrogen and oxygen. This technology is seen as an important way to achieve sustainable energy because hydrogen is a clean fuel that can generate electricity through hydrogen fuel cells and only releases water vapor during combustion, without producing greenhouse gases such as carbon dioxide.
[0003] Electrocatalytic water splitting usually consists of two parts, the hydrogen evolution reaction (HER) at the cathode to produce hydrogen and the oxygen evolution reaction (OER) at the anode to produce oxygen. However, in practical applications, since OER involves a four-electron transfer reaction and needs to overcome the huge activation energy barrier of OH bond breaking and O–O double bond formation, while HER only involves a two-electron transfer reaction. In order to overcome the sluggish kinetics of OER, various studies have been conducted to design electrocatalysts to promote the process. Currently, the most ideal HER and OER catalysts are Pt-based and Ir, Ru-based precious metal catalysts, respectively, but their expensive and scarce properties make them impossible for large-scale commercial applications. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a preparation method and application of a polysulfide polymer intercalated nickel-molybdenum double metal hydroxide composite material with excellent electrocatalytic hydrogen and oxygen evolution performance.
[0005] The technical solution adopted by the present invention to solve the above technical problems is: a method for preparing a polysulfide polymer intercalated nickel-molybdenum double metal hydroxide composite material, comprising the following steps:
[0006] (1) Prepare needle-shaped NiMo double transition metal hydroxide on a support by a hydrothermal method, denoted as NiMo-LDH / NF;
[0007] (2) preparing polysulfide polymers containing rigid segments by polymerizing monomers through a reverse vulcanization method;
[0008] (3) The polysulfide polymer obtained in step (2) is intercalated into the NiMo-LDH / NF material obtained in step (1) by a hydrothermal method and subjected to sulfurization, so that the sulfur in the polysulfide polymer replaces the hydroxide, thereby obtaining a polysulfide polymer intercalated nickel-molybdenum double metal hydroxide composite material, which is recorded as Mo-Ni2S3 / NF-monomer.
[0009] Furthermore, step (1) is specifically as follows: adding the pretreated flaky nickel foam to a mixed solution consisting of a nickel source, a molybdenum source and an ammonium source, and then reacting in a high-pressure reactor at a reaction temperature of 120-180°C and a reaction pressure of 2-6.5 bar for 8-15 hours, cooling to room temperature, washing and drying to obtain a nickel foam loaded with needle-shaped NiMo double transition metal hydroxide.
[0010] Furthermore, the nickel source is selected from any one of nickel nitrate, nickel chloride or nickel sulfate; the molybdenum source is selected from any one of sodium molybdate, ammonium molybdate or calcium molybdate; the ammonium source is selected from any one or any two of urea, ammonium fluoride, ammonium chloride or ammonium nitrate; and the solvent is any one of water, ethanol or methanol.
[0011] Furthermore, the molar ratio of the nickel foam area to the nickel source is (2.7-3.3) cm 2 :1mmol, the concentration of nickel source in the mixed solution is 0.02-0.04mol / L; the molar ratio of nickel source to molybdenum source is (5-10):1; the molar ratio of ammonium source to nickel source is (2-5):1.
[0012] Further, step (2) is as follows: adding the polymerizable monomer and sublimed sulfur in a mass ratio of (9-4):1 into a test tube, heating the test tube to a temperature of 160-190°C, polymerizing for 0.5-8 hours, and then heating in a water bath at 70-90°C to dissolve in a polar solvent to obtain a polysulfide polymer solution, wherein the polysulfide polymer solution has a sulfur content of 0.06-0.065 mol / L. Principle of reverse sulfidation reaction: sulfur diradicals act as initiators and organic monomers act as crosslinking agents to form new polysulfides.
[0013] Furthermore, the polymerization monomer is selected from any one of biphenyl-4,4'-dithiol (BDP), resorcinol (1,3-BDT), hydroquinone (1,4-BDT), diisopropenylbenzene (DIB), vinyl norbenzene (VDB) or dicyclopentadiene (DCPD); and the polar solvent is selected from any one of N,N-dimethylformamide, N,N-dimethylacetamide and tetrahydrofuran.
[0014] Furthermore, step (3) is specifically as follows: the NiMo-LDH / NF composite material obtained in step (1) and the polysulfide polymer solution obtained in step (2) are added into an autoclave, reacted at 160-200° C. for 8-12 h, cooled to room temperature, washed and dried to obtain a polysulfide polymer intercalated nickel-molybdenum double hydroxide composite material, recorded as Mo-Ni2S3 / NF-monomer, wherein the molar ratio of sulfur in the polysulfide polymer to molybdenum in the molybdenum source is (2-3):10.
[0015] The present invention also provides an application of the polysulfide polymer intercalated nickel-molybdenum double metal hydroxide composite material prepared by the above preparation method in the preparation of electrocatalytic oxygen evolution and / or hydrogen evolution catalysts.
[0016] Compared with the prior art, the advantages of the present invention are:
[0017] 1) The composite catalytic material prepared by the present invention grows on the surface of the nickel foam skeleton structure and can be directly used as an electrode as a self-supported catalyst;
[0018] 2) Using nano-needle NiMo-LDH as a template, sulfur atoms are discretely loaded on the original nano-needle structure after polysulfide polymer vulcanization, which increases the specific surface area of the material and improves the electron and proton transport capabilities of the material;
[0019] 3) Based on the polysulfide polymer intercalation method, the present invention generates a mixed crystal structure and a metastable 1T phase by a hydrothermal method using a bulky polysulfide polymer. The bulky polysulfide polymer disrupts and expands the original arrangement of the composite catalytic material, thereby avoiding the superposition of two-dimensional material layers, increasing the specific surface area, and achieving the purpose of increasing the number of active sites;
[0020] 4) The electrocatalyst composite material Mo-Ni2S3 / NF-monomer obtained by the preparation method of the present invention has excellent electrocatalytic oxygen evolution performance under alkaline conditions, 10 mA cm -2 At current density, the overpotential is 105 mV; 50 mA cm -2 At current density, the overpotential is 210 mV. The ammonium source used can regulate the material morphology, deposition rate, bath stability, deposition quality and corrosion resistance;
[0021] 5) Based on the template method, the obtained catalyst structure is stable, which can prevent accidental aggregation during the electrochemical process, enhance the electron donor ability, promote electrode kinetics, and increase the number of active sites;
[0022] 6) Depending on the monomers used, reactions such as chain growth, proton transfer, chain transfer and dynamic exchange of disulfide bonds may occur between monomers, thus forming a complex branched structure. During the catalyst preparation process, it acts as a template and bridging agent to expand the original stacked layers of the catalyst, increase the electrocatalytic active sites, and simultaneously undergo secondary structural reconstruction to obtain electrocatalysts with different microscopic morphologies. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A flow chart for the preparation of nickel-molybdenum double hydroxide composites intercalated with polysulfide polymers;
[0024] Figure 2 is the XRD diffraction pattern of Mo-Ni2S3 / NF-BDP;
[0025] Figure 3 It is the XPS spectrum of Mo-Ni2S3 / NF-1,3-BDT;
[0026] Figure 4 Schematic diagram of the structure of the polysulfide polymer prepared by the inverse vulcanization method in Examples 1-3;
[0027] Figure 5 (a), (b), (c) SEM images of NiMo-LDH / NF, (d) SEM image of Mo-Ni2S3 / NF-1,3-BDT, (e) SEM image of Mo-Ni2S3 / NF-1,4-BDT, (f) SEM image of Mo-Ni2S3 / NF-BDP, (g) SEM image of Mo-Ni2S3 / NF-S;
[0028] Figure 6 (a) HER LSV curves and (b) OER LSV curves of Mo-Ni2S3 / NF-BDP, Mo-Ni2S3 / NF-1,3-BDT, Mo-Ni2S3 / NF-1,4-BDT and Mo-Ni2S3 / NF-S;
[0029] Figure 7 (a) Tafel slope curves and (b) Nyquist plots of Mo-Ni2S3 / NF-BDP, Mo-Ni2S3 / NF-1,3-BDT, Mo-Ni2S3 / NF-1,4-BDT and Mo-Ni2S3 / NF-S;
[0030] Figure 8 Cyclic voltammograms of Mo-Ni2S3 / NF-1,3-BDT (a), Mo-Ni2S3 / NF-1,4-BDT (b), Mo-Ni2S3 / NF-S (c) and Mo-Ni2S3 / NF-BDP (d); (e) the electrochemically active surface area (ECSA) was estimated by fitting a linear regression by plotting the relationship between current density and scan rate;
[0031] Fig. 9 (a) is the full water splitting device and (b) is the double hydrolysis voltammetric characteristic curves of Mo-Ni2S3 / NF-BDP, Mo-Ni2S3 / NF-1,3-BDT, Mo-Ni2S3 / NF-1,4-BDT and Mo-Ni2S3 / NF-S. DETAILED DESCRIPTION
[0032] The present invention is further described in detail below with reference to the accompanying drawings. Specific embodiments
[0033] Example 1: A polysulfide polymer intercalated nickel-molybdenum double hydroxide composite material Mo-Ni2S3 / NF-BDP, prepared by the following method: Figure 1 As shown, the following steps are included:
[0034] 1. A 3 cm × 1 cm nickel foam was ultrasonically treated in 3 M HCl solution, anhydrous ethanol and deionized water for 15 min to remove possible oxides on the surface, and then washed with ultrapure water for several times and dried for later use. The treated nickel foam was placed in 40 mL deionized water containing 6.9 mmol Ni(NO3)2·6H2O, 0.68 mmol Na2MoO4·2H2O, 10 mmol urea and 5 mmol NH4F, and the mixed solution was transferred to a 50 mL stainless steel autoclave lined with polytetrafluoroethylene, and reacted at 180 ° C in a muffle furnace for 10 h. After the reaction was cooled to room temperature, the nickel foam was taken out, rinsed repeatedly with ethanol and deionized water several times, and then placed in a freeze dryer for 12 h to obtain NiMo-LDH / NF.
[0035] 2. Weigh 0.0889 g of biphenyl-4,4'-dithiol (BDP) and 0.9 g of sublimed sulfur (S8), grind them in a mortar until they are evenly mixed, transfer them to a test tube, put in a small magnetic stirring bar, and then place them in a dimethyl silicone oil bath and heat them to 160 °C. When clear yellow molten sulfur is formed, heat it to 200 °C and continue stirring. After stirring with a small magnetic stirring bar for about 6 hours, the yellow solution turns into a red vitrified medium, and conjugated chain polysulfide polymers are obtained after cooling.
[0036] 3. Dissolve the prepared polysulfide polymer in DMF solvent in a 90 °C water bath to prepare a polysulfide polymer solution. Dilute the polysulfide polymer solution with DMF to a sulfur concentration of 0.0625 mol L -1 The prepared NiMo-LDH / NF was placed in the autoclave and heated at 180 °C for 10 h in an oven and then cooled to room temperature naturally. The synthesized sample was rinsed with deionized ethanol / water several times and placed in a freeze dryer for 12 h to obtain the Mo-Ni2S3 / NF-BDP catalytic electrode.
[0037] The XRD characteristics of the Mo-Ni2S3 / NF-BDP composite material prepared in Example 1 are shown in FIG. Figure 2 ,like Figure 2 As shown in Figure 2, the XRD pattern confirmed the successful synthesis of NiMo-LDH. NiMo-LDH / NF 。 , 29.86 。 and 33.41 。The obvious diffraction peak at 44.58 is consistent with the NiMoO4.xH2O standard card (PDF#13-0128), while the 。 , 52.02 。 and 76.50 。 The peak at 27.33 belongs to NF, which indicates that NiMo-LDH has been synthesized and attached to NF. After polysulfide sulfidation, some characteristic peaks of NiMo-LDH / NF disappeared, such as 27.33 。 The peaks at 21.75 and 22.75 cm are replaced by some new peaks, which are in good agreement with the standard charts of Ni S32 (PDF#44-1418) and Mo S159 (PDF#40-0936). 。 , 31.10 。 , 49.73 。 and 55.16 。 The characteristic peaks at are assigned to the (101), (110), (113) and (122) lattice planes of Ni3S2 (PDF#44-1418); for Mo 15 S9, at 35.77 。 and 41.07 。 The characteristic peaks are attributed to Mo 15 The (124) and (131) lattice planes of S9 (PDF#40-0936) imply that the process of sulfiding NiMo-LDH is successful.
[0038] Example 2: Preparation of Mo-Ni2S3 / NF-1,3-BDT material
[0039] 1. A 3 cm × 1 cm nickel foam was ultrasonically treated in 3 M HCl solution, anhydrous ethanol and deionized water for 15 min respectively to remove possible oxides on the surface, and then washed with ultrapure water for several times and dried for later use; the treated nickel foam was placed in 40 mL deionized water containing 6.9 mmol Ni(NO3)2·6H2O, 0.68 mmol Na2MoO4·2H2O, 10 mmol urea and 5 mmol NH4F, and the mixed solution was transferred to a 50 mL stainless steel autoclave lined with polytetrafluoroethylene, and reacted at 180 ℃ in a muffle furnace for 10 h. After the reaction was cooled to room temperature, the nickel foam was taken out, rinsed repeatedly with ethanol and deionized water several times, and then dried in a freeze dryer for 12 h to obtain NiMo-LDH / NF.
[0040] 2. Weigh 0.0889 g of isophthalic acid dithiol (1,3-BDT) and 0.9 g of sublimed sulfur (S8), grind them in a mortar until they are evenly mixed, transfer them to a test tube, put in a small magnetic stirring bar, and then place them in a dimethyl silicone oil bath and heat them to 160 °C. When clear yellow molten sulfur is formed, heat it to 200 °C and continue stirring. After stirring with a small magnetic stirring bar for about 6 hours, the yellow solution turns into a red vitrified medium, and conjugated chain polysulfide polymers are obtained after cooling.
[0041] 3. Dissolve the prepared polysulfide polymer in DMF solvent in a 90 °C water bath to prepare a polysulfide polymer solution. Dilute the polysulfide polymer solution with DMF to a sulfur concentration of 0.0625 mol L -1 The prepared NiMo-LDH / NF was placed in the autoclave and heated at 180°C for 10 h in an oven and then cooled to room temperature naturally. The synthesized sample was rinsed with deionized ethanol / water several times and placed in a freeze dryer for 12 h to obtain the Mo-Ni2S3 / NF-1,3-BDT catalytic electrode.
[0042] The XPS of Mo-Ni2S3 / NF-1,3-BDT composite material prepared in Example 2 is shown in Figure 3 ,like Figure 3 As shown in Figure 2, the prepared composite electrocatalytic electrode contains Ni, Mo, S and O elements, and the sulfur element comes from the sulfur in the polysulfide polymer. In the Ni 2p spectrum, Ni 2+ 2p and Ni 3+ 2p orbital peaks, they can detect two spin-orbit peaks and two satellite peaks, Ni 2+ 2p 1 / 2 and Ni 2+ 2p 3 / 2 The peaks of Ni are located at 873.28eV and 855.89eV. 3+ 2p 1 / 2 and Ni 3+ 2p 3 / 2 The peaks of MoS23d and Mo are located at 876.17eV and 857.91eV. 6+ The two spin-orbit peaks are located at 232.12eV and 228.94eV and 235.26eV and 231.63eV respectively. In addition, the S 2p peak at 226.17 eV indicates that the sulfur in MoS2 is in the form of S 2- This is different from the molybdenum element in MoS2 being in the form of Mo 4+In the S 2d spectrum, orbital peaks of Ni2S3 and MoS2 appear, and their two spin-orbit peaks are located at 164.83eV and 163.71eV and 162.07eV and 161.45eV. Combined with the peak area in the spectrum, it can be explained that the nickel-molybdenum sulfides in Mo-Ni2S3 / NF-1,3-BDT mainly exist in the form of Ni2S3 and MoS2, with some MoS3 attached, which also shows that NiMo-LDH has been successfully sulfurized. The Ni 2p spectrum of Ni 3+ The presence of is due to the partial oxidation of the sample by oxygen in the air, which is consistent with the O 2p spectrum occupying the largest peak area. 2 The peaks are consistent.
[0043] Example 3: Preparation of Mo-Ni2S3 / NF-1,4-BDT material
[0044] 1. A 3 cm × 1 cm nickel foam was ultrasonically treated in 3 M HCl solution, anhydrous ethanol and deionized water for 15 min respectively to remove possible oxides on the surface, and then washed with ultrapure water for several times and dried for later use; the treated nickel foam was placed in 40 mL deionized water containing 6.9 mmol Ni(NO3)2·6H2O, 0.68 mmol Na2MoO4·2H2O, 10 mmol urea and 5 mmol NH4F, and the mixed solution was transferred to a 50 mL stainless steel autoclave lined with polytetrafluoroethylene, and reacted at 180 ℃ in a muffle furnace for 10 h. After the reaction was cooled to room temperature, the nickel foam was taken out, rinsed repeatedly with ethanol and deionized water several times, and then dried in a freeze dryer for 12 h to obtain NiMo-LDH / NF.
[0045] 2. Weigh 0.0889 g of 1,4-BDT and 0.9 g of sublimed sulfur (S8), grind them in a mortar until they are evenly mixed, transfer them to a test tube, put in a small magnetic stirring bar, and then heat them in a dimethyl silicone oil bath to 160 ° C. When clear yellow molten sulfur is formed, heat it to 200 ° C and continue stirring. After stirring with a small magnetic stirring bar for about 6 hours, the yellow solution turns into a red vitrified medium, and conjugated chain polysulfide polymers are obtained after cooling.
[0046] 4. Dissolve the prepared polysulfide polymer in DMF solvent in a 90 °C water bath to prepare a polysulfide polymer solution. Dilute the polysulfide polymer solution with DMF to a sulfur concentration of 0.0625 mol L -1The prepared NiMo-LDH / NF was placed in the autoclave and heated at 180°C for 10 h in an oven and then cooled to room temperature naturally. The synthesized sample was rinsed with deionized ethanol / water several times and dried in a freeze dryer for 12 h to obtain the Mo-Ni2S3 / NF-1,4-BDT catalytic electrode.
[0047] In the above examples 1-3, biphenyl-4,4'-dithiol (BDP), resorcinol dithiol (1,3-BDT), and hydroquinone dithiol (1,4-BDT) are used as polymerization monomers and molten sublimed sulfur is used as solvent. The polysulfide polymer structure is as follows: Figure 4 shown.
[0048] In addition to the above embodiments, the nickel source in step (1) can also be selected from nickel chloride or nickel sulfate; the molybdenum source can also be selected from ammonium molybdate or calcium molybdate; the ammonium source can also be selected from one ammonium chloride, one ammonium nitrate, two kinds of urea and ammonium chloride, two kinds of urea and ammonium nitrate, two kinds of ammonium fluoride and ammonium chloride, and two kinds of ammonium fluoride and ammonium nitrate; the solvent can also be ethanol or methanol. The molar ratio of the area of the nickel foam to the nickel source can also be (2.7-3.3) cm 2 : any value within 1mmol; the concentration of the nickel source in the mixed solution is any value within 0.02-0.04mol / L; the molar ratio of the nickel source to the molybdenum source is any value within (5-10):1; the molar ratio of the ammonium source to the nickel source is any value within (2-5):1.
[0049] In step (2), the polymerization monomer may be selected from any one of diisopropenylbenzene (DIB), vinyl norbenzene (VDB) or dicyclopentadiene (DCPD); the polar solvent is selected from any one of N,N-dimethylformamide, N,N-dimethylacetamide and tetrahydrofuran; the mass ratio of the polymerization monomer to the sublimated sulfur is any value within the range of (9-4):1; and the sulfur content in the polysulfide polymer solution is any value within the range of 0.06-0.065 mol / L.
[0050] In step (3), the molar ratio of sulfur in the polysulfide polymer to molybdenum in the molybdenum source is any value within the range of (2-3):10.
[0051] Comparative Example: Steps for preparing Mo-Ni2S3 / NF-S material:
[0052] 1. A 3 cm × 1 cm nickel foam was ultrasonically treated in 3 M HCl solution, anhydrous ethanol and deionized water for 15 min respectively to remove possible oxides on the surface, and then washed with ultrapure water for several times and dried for later use; the treated nickel foam was placed in 40 mL deionized water containing 6.9 mmol Ni(NO3)2·6H2O, 0.68 mmol Na2MoO4·2H2O, 10 mmol urea and 5 mmol NH4F, and the mixed solution was transferred to a 50 mL stainless steel autoclave lined with polytetrafluoroethylene, and reacted at 180 ℃ in a muffle furnace for 10 h. After the reaction was cooled to room temperature, the nickel foam was taken out, rinsed repeatedly with ethanol and deionized water several times, and then dried in a freeze dryer for 12 h to obtain NiMo-LDH / NF.
[0053] 2. Weigh 0.9 g of sublimed sulfur (S8), add 50 ml of DMF and heat in a water bath until it is completely dissolved.
[0054] 3. Dilute the DMF solution of sublimated sulfur with DMF to a sulfur concentration of 0.0625 mol L -1 The prepared NiMo-LDH / NF was placed in the autoclave and heated at 180°C for 10 h in an oven and then cooled to room temperature naturally. The synthesized sample was rinsed with deionized ethanol / water several times and placed in a freeze dryer for 12 h to obtain the Mo-Ni2S3 / NF-S catalytic electrode.
[0055] 2. Experimental Results Analysis
[0056] 1. SEM characterization of Mo-Ni2S3 / NF-monomer composites
[0057] The SEM images of the composite materials of the polysulfide polymer intercalated nickel-molybdenum double hydroxide and the support prepared in Examples 1, 2 and 3 are shown in FIG. Figure 5 .like Figure 5 As shown in Figure 5 (a) (b) (c) shows the NiMo-LDH / NF surface at different magnifications, the densely arranged nano-needle structure can be clearly seen, which leads to a higher specific surface area and thus provides more active sites. After polysulfide sulfurization, sulfur atoms are densely loaded on NiMo-LDH. The sulfur atoms on the surface of Mo-Ni2S3 / NF-1,3-BDT are concentrated on the needle-shaped NiMo-LDH ( Figure 5 d), while the sulfur atoms on the surface of Mo-Ni2S3 / NF-1,4-BDT are connected in a linear manner ( Figure 5e). On the surface of Mo-Ni2S3 / NF-BDP, sulfur atoms are densely loaded at the roots of the needle-like NiMo-LDH nanorods, thus constructing a needle-like network structure ( Figure 5 f). However, the sulfur atoms generated by the sulfurization of small molecules filled the gaps between the nanoneedle-shaped NiMo-LDH in a disordered and high-density stacking manner ( Figure 5 g). This difference illustrates the difference in the structural assembly of small and large molecular sulfur during the sulfurization process. The different surfaces are related to the structure of the monomers. The polysulfides bound to Mo-Ni2S3 / NF-1,3-BDT and Mo-Ni2S3 / NF-1,4-BDT present a linear structure, which is consistent with Figure 5 d and Figure 5 e. In contrast, due to the larger and more complex structure of Mo-Ni2S3 / NF-BDP, the polysulfides derived from Mo-Ni2S3 / NF-BDP formed a dispersed embedded structure, such as Figure 5 f shown.
[0058] Hydrogen and oxygen evolution properties of Mo-Ni2S3 / NF-monomer composites
[0059] The electrochemical tests were all carried out on a Chenhua 760E electrochemical workstation. A standard three-electrode system was used in the test, with a piece of newly prepared electrode material directly used as the working electrode, a graphite rod used as the counter electrode, and a saturated calomel electrode used as the reference electrode. The test temperature was 25 °C, and the electrolyte during the test was 1 M KOH saturated with N2. In the test, the external voltage applied for the HER test was -1.5—-0.9 V, and the external voltage applied for the OER test was 0-0.7 V. The overpotential of the Mo-Ni2S3 / NF-monomer composite material was obtained after processing according to the Nernst equation.
[0060] The LSV of the composite material of the polysulfide polymer intercalated nickel-molybdenum double hydroxide and the support prepared in Examples 1, 2 and 3 is shown in FIG. Figure 6 .like Figure 6 As shown in a, the HER performance of Mo-Ni2S3 / NF-monomer, Mo-Ni2S3 / NF-S and NiMo-LDH / NF obtained by sulfurization of polysulfide polymers prepared based on monomers BDP, 1,3-BDT and 1,4-BDT was measured by LSV test at a current density of 10 mA / cm 2 When the current density is 50 mA / cm 2 When the overpotential is 289 mV, 252 mV, 205 mV, 331 mV and 381 mV respectively. The LSV test measurement results of OER performance are shown in Figure 6As shown in b, at a current density of 10 mA / cm 2 When the current density is 50 mA / cm 2 When the overpotential is 210 mV, 141 mV, 132 mV, 343 mV and 403 mV, respectively. By comparing the HER and OER performance data of Mo-Ni2S3 / NF-monomer and NiMo-LDH / NF, the results show that the HER and OER performance of NiMo-LDH are significantly improved after sulfurization compared with the reduced oxidation state (SOR). However, there are also significant differences in the performance of the composites obtained from different sulfur sources, especially in the selection of small monomer sulfur sources and macromolecular sulfur sources. This shows that polysulfide, as a macromolecule, can not only play a role in improving performance through SOR, but also has a positive effect on the construction of the composite structure.
[0061] The specific preparation steps of the noble metal oxygen evolution reference sample RuO2 / NF catalytic electrode are as follows: First, 4 mgRuO2 and 20 μL Nafion solution (5 wt%) are dispersed in 980 μL deionized water and ethanol (V 水 / V 乙醇 =2:1) and subjected to ultrasonic treatment for 1h. Then, 500 μL of uniform dispersion was added to the NF surface and infrared dried at room temperature for storage. In addition, the noble metal hydrogen evolution reference sample Pt / C / NF was prepared by drop coating. 4 mgPt / C and 40 μL Nafion solution (5 wt%) were dispersed in 960 μL solvent (720 μL ultrapure water and 240 μL ethanol). After ultrasonic treatment for 1 hour, the electrocatalyst ink was uniformly coated on the NF (0.5 cm×0.5 cm) and heated at 50 ◦ C vacuum drying for 10 hours.
[0062] RuO2 / NF is a typical noble metal oxygen evolution electrocatalyst with a current density of 10 mA / cm 2 When the overpotential is 235.4 mV, Pt / C / NF is a typical noble metal hydrogen evolution electrocatalyst with a current density of 10 mA / cm 2 and 50 mA / cm 2 The overpotentials are 42 mV and 89 mV, respectively. The above results show that Mo-Ni2S3 / NF-monomer composites prepared based on non-precious metal sulfides have great potential to replace precious metal electrocatalysts.
[0063] 3. Impedance performance of Mo-Ni2S3 / NF-monomer composite materials
[0064] The Tafel slope and EIS of the composite material of the polysulfide polymer intercalated nickel-molybdenum double hydroxide and the support prepared in Examples 1, 2, 3 and Comparative Example are shown in FIG. Figure 7 .like Figure 7 As shown in Figure 1, the Mo-Ni2S3 / NF-BDP catalyst has the lowest Tafel slope of 36.11 mV / dec, compared with other catalysts Mo-Ni2S3 / NF-1,3-BDT (49.12 mV / dec), Mo-Ni2S3 / NF-1,4-BDT (47.17 Mv / dec), Mo-Ni2S3 / NF-S (189.10 mV / dec), and NiMo-LDH (140.72 mV / dec). It is worth noting that the Mo-Ni2S3 / NF-monomer composites mediated by polysulfide sulfurization exhibit lower Tafel slope values, indicating that the nanostructures of these catalysts present a 1T phase. In previous studies using thiourea for sulfurization, the Tafel slopes of the target samples have always been higher than those of Mo-Ni2S3 / NF-BDP. The smaller Tafel slope indicates better kinetic performance of the HER and OER processes, which means that the catalyst surface based on the Mo-Ni2S3 / NF-BDP macromolecular sulfur source can provide more active sites, thereby improving the catalytic performance. Figure 7 As shown in (b), the equivalent series resistance of Mo-Ni2S3 / NF-BDP is 7.89Ω, which is higher than that of Mo-Ni2S3 / NF-1,3-BDT (7.43Ω), Mo-Ni2S3 / NF-1,4-BDT (6.67Ω) and Mo-Ni2S3 / NF-S (7.57Ω). However, Mo-Ni2S3 / NF-BDP shows the smallest semicircle diameter, indicating that the charge transfer resistance is smaller than that of other composites. This is consistent with the performance of the Tafel plot. In addition, compared with Mo-Ni2S3 / NF-S, the semicircle diameter of Mo-Ni2S3 / NF-monomer composites mediated by polysulfide sulfurization is generally much smaller, which is related to the unique surface structure formed by polysulfides. This may be due to the random distribution caused by the disordered stacking of small sulfur molecules between NiMo-LDH, resulting in the weakening of the electron transport ability of Mo-Ni2S3 / NF-S.
[0065] 4. Full water splitting performance of Mo-Ni2S3 / NF-monomer composite materials
[0066] The ECSA of the composite material of the polysulfide polymer intercalated nickel-molybdenum double hydroxide and the support prepared in Examples 1, 2 and 3 is shown in Figure 8 .like Figure 8 As shown, using cyclic voltammetry (CV) technique, C dlThe electrochemical surface area (ECSA) of Mo-Ni2S3 / NF was calculated. The CV curves of Mo-Ni2S3 / NF-1,3-BDT, Mo-Ni2S3 / NF-1,4-BDT, Mo-Ni2S3 / NF-BDP and Mo-Ni2S3 / NF-S in the potential region of 0.1 V to RHE are shown in ( Figure 8 ad). By plotting the different anodic and cathodic current densities at 0.2 V versus different scan rates (20-100 mV / s). dl like Figure 8 As shown in e, the ECSA of Mo-Ni2S3 / NF-BDP is 7.56 mF / cm 2 , greater than Mo-Ni2S3 / NF-1,3-BDT (6.72mF / cm 2 ), Mo-Ni2S3 / NF-1,4-BDT (5.69mF / cm 2 ) and Mo-Ni2S3 / NF-S (4.93mF / cm 2 ). This indicates that Mo-Ni2S3 / NF-BDP has a larger ECSA and can provide more active sites compared to Mo-Ni2S3 / NF-1,3-BDT, Mo-Ni2S3 / NF-1,4-BDT, and Mo-Ni2S3 / NF-S. It is also worth noting that Mo-Ni2S3 / NF-monomers mediated by polysulfide sulfurization generally exhibit larger ECSAs than Mo-Ni2S3 / NF-S obtained by sulfurization of NiMo-LDH / NF with a small molecule sulfur source. This phenomenon can be explained by the lack of rigid structure of small molecule sulfur, which is prone to high-density aggregation, thus masking the active sites. In contrast, the rigid fragments of polysulfides can provide more active sites compared to powdered sulfur due to their self-supporting structure.
[0067] 5. Full water splitting performance of Mo-Ni2S3 / NF-monomer composite materials
[0068] The overall water splitting performance of the composite material of the polysulfide polymer intercalated nickel-molybdenum double hydroxide and the support prepared in Examples 1, 2, and 3 is shown in Fig. 9 As shown, the voltage set for the test is 1-2 V. Cut two 1 cm 2 The Mo-Ni2S3 / NF-monomer composites prepared in each example were used as anode and cathode at the same time, and an overall full water splitting device was assembled in 1M KOH ( Fig. 9 a). Fig. 9 As shown in b, when the current density is 100 Ma / cm 2When the voltage applied by Mo-Ni2S3 / NF-BDP is 1.672V, which is lower than the voltage applied by Examples 2 and 3 (1.693 V and 1.718 V) and Mo-Ni2S3 / NF-S (1.802 V). This voltage value is lower than most non-precious transition metal electrocatalysts reported recently, which indicates that Mo-Ni2S3 / NF-BDP has good practical application prospects. In industrial production, the Mo-Ni2S3 / NF-BDP composite material prepared by this method can be used as an electrocatalyst for both the positive and negative electrodes of the electrolyzer, which is conducive to the unified procurement and management of catalysts by the factory.
[0069] In summary, the present invention obtains the Mo-Ni2S3 / NF composite material by performing hydrothermal reaction, calcination treatment and in-situ sulfidation on nickel foam, and has excellent electrocatalytic hydrogen and oxygen evolution performance under alkaline conditions.
[0070] The above description is not intended to limit the present invention, and the present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by a person skilled in the art within the spirit and scope of the present invention shall also fall within the protection scope of the present invention.
Claims
1. A method for preparing a polysulfide polymer intercalated nickel-molybdenum double hydroxide composite material, Features The following steps are involved: (1) A needle-shaped NiMo double transition metal hydroxide (NiMo-LDH / NF) was prepared on a support by a hydrothermal method, as follows: the pretreated flaky nickel foam was added to a mixed solution consisting of a nickel source, a molybdenum source and an ammonium source, and then reacted in a high-pressure reactor at a temperature of 120-180°C and a pressure of 2-6.5 bar for 8-15 h, cooled to room temperature, washed and dried to obtain a nickel foam loaded with a needle-shaped NiMo double transition metal hydroxide, wherein the molar ratio of the area of the nickel foam to the nickel source was (2.7-3.3) cm 2 :1mmol, the concentration of nickel source in the mixed solution is 0.02-0.04mol / L; the molar ratio of nickel source to molybdenum source is (5-10):1; the molar ratio of ammonium source to nickel source is (2-5):1; (2) preparing a polysulfide polymer containing a rigid segment from a polymerized monomer by a reverse vulcanization method, specifically as follows: adding the polymerized monomer and sublimed sulfur in a mass ratio of (9-4):1 into a test tube, heating the test tube to a temperature of 160-190°C, performing a polymerization reaction for 0.5-8 hours, and then heating in a water bath at 70-90°C to dissolve the polymer in a polar solvent to obtain a polysulfide polymer solution, wherein the sulfur content of the polysulfide polymer solution is 0.06-0.065 mol / L, wherein the polymerized monomer is selected from any one of biphenyl-4,4'-dithiol, resorcinol, and hydroquinone; and the polar solvent is selected from any one of N,N-dimethylacetamide, N,N-dimethylacetamide, and tetrahydrofuran; (3) The polysulfide polymer obtained in step (2) is intercalated into the NiMo-LDH / NF material obtained in step (1) by a hydrothermal method for sulfurization, and the sulfur in the polysulfide polymer replaces the hydroxide to obtain a polysulfide polymer intercalated nickel-molybdenum double hydroxide composite material, specifically as follows: the NiMo-LDH / NF composite material obtained in step (1) and the polysulfide polymer solution obtained in step (2) are added to an autoclave, reacted at 160-200° C. for 8-12 h, cooled to room temperature, washed and dried, to obtain a polysulfide polymer intercalated nickel-molybdenum double hydroxide composite material, recorded as Mo-Ni 2 S 3 / NF-monomer, wherein the molar ratio of sulfur in the polysulfide polymer to molybdenum in the molybdenum source is (2-3):
10.
2. A method for preparing a polysulfide polymer intercalated nickel-molybdenum double hydroxide composite material according to claim 1, Features: The nickel source is selected from any one of nickel nitrate, nickel chloride or nickel sulfate; the molybdenum source is selected from any one of sodium molybdate, ammonium molybdate or calcium molybdate; the ammonium source is selected from any one or any two of urea, ammonium fluoride, ammonium chloride or ammonium nitrate; and the solvent is any one of water, ethanol or methanol.
3. Use of a polysulfide polymer intercalated nickel-molybdenum double metal hydroxide composite material prepared by the preparation method according to any one of claims 1 to 2 in the preparation of electrocatalytic oxygen evolution and hydrogen evolution catalysts.
Citation Information
Patent Citations
Ni-Co double metal hydroxide nanometer sheet / N-doped carbon fiber hybrid material and preparation method thereof
CN105513819A
Transition metal sulfide electrode material based on sulfur chain polymers, preparation method of material and application of material
CN110304657A
Caterpillar-shaped nickel-cobalt sulfide nano array as well as synthesis and application thereof
CN111604061A
Electrolyzed water material with heterojunction structure as well as preparation method and application of electrolyzed water material
CN113957474A
Carbon-supported CoFe bimetallic sulfide electrode material, preparation method and application
CN117926337A