A kind of flexible high-strength composite fabric and preparation method thereof

Through plasma treatment and chemical modification technology, the bonding strength and performance of wool fiber and polyester fiber are improved, and the problems of wool fiber shrinking and deforming and polyester fiber losing elastic recovery ability are solved, and a fiber with high strength and good resistance is prepared. Flexible and high-strength composite fabric with excellent flammability.

CN118498085BActive Publication Date: 2024-10-01杭州大统纺织有限公司
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410978763.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-01
Estimated Expiration
2044-07-22

AI Technical Summary

Technical Problem

Wool fiber is prone to felting and hairiness under friction or alkaline conditions, resulting in reduced fabric size and chaotic texture, which limits its application areas. Polyester fiber loses its elastic recovery ability at high temperatures, affecting the shape retention of clothing.

Method used

Wool fibers and polyester fibers are surface treated by plasma to form micropores and slits to increase physical anchoring points, and are modified with chemicals such as dopamine hydrochloride and epichlorohydrin to increase flame retardant and antibacterial properties, combined with carboxymethyl Chitosan and blocked isocyanate cross-linking agent are used for cross-linking to improve the mechanical strength and hygroscopicity of the fabric.

Benefits of technology

The preparation of flexible high-strength composite fabrics has been achieved, the flame retardant, antibacterial properties and mechanical strength of the fabrics have been improved, the soft skin-friendly and flame retardant effects of the fabrics have been enhanced, and the problem of wool fibers easily shrinking and deforming has been solved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a flexible high-strength composite fabric and a preparation method thereof. The invention can form micropores and slits on the fiber surface by plasma treatment of wool fiber and polyester fiber, thereby providing more physical anchoring points; at the same time, the plasma treatment can activate the fiber surface, introduce polar functional groups such as carboxyl and hydroxyl groups, and facilitate subsequent reactions; dopamine is used to modify the wool fiber, and a polydopamine layer is deposited on the surface of the wool fiber. After the wool fiber is modified by polydopamine, amino active functional groups are introduced, which is conducive to subsequent reactions. At the same time, polydopamine has excellent flame retardant properties, and its introduction into the composite fabric is conducive to improving the flame retardant properties of the fabric; at the same time, guanidine sulfonate is grafted onto the polyester fiber through the cross-linking effect of epichlorohydrin. Guanidine sulfonate has excellent antibacterial properties and flame retardant properties, and its introduction into the composite fabric enhances the antibacterial properties and flame retardant properties of the fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textile fabrics, and in particular to a flexible high-strength composite fabric and a preparation method thereof. Background Art

[0002] Woolen fabric, also known as wool fabric, is a kind of fabric made of wool as the main raw material through textile technology. Woolen fabric is widely used in the manufacture of formal and high-end clothing such as dresses, suits, coats, etc. due to its excellent warmth retention, comfort and beauty. At the same time, it also has certain applications in home textiles, toys, bags and other fields.

[0003] There is a layer of scales on the surface of wool fibers, just like fish scales or tiles on the roof. When the wool fibers are rubbed or rubbed, they will tangle with each other and feel together. Increasing the temperature or under alkaline conditions will intensify this reaction. When washed, the wool fibers are constantly squeezed and rubbed, and the felt will shrink, causing changes in the fabric size, hairiness, and disordered texture. The continuous accumulation of the above changes will affect the appearance and wearing performance of the fabric, and to a certain extent limit the application areas of wool.

[0004] Polyester fiber is a synthetic fiber obtained by spinning polyester obtained by polycondensation of polyols and polyacids. It is referred to as PET fiber. It is a polymer compound. Polyester fiber has excellent wear resistance, which enables polyester fiber products to maintain good appearance and performance after long-term use. At the same time, polyester fiber has high elastic recovery ability, so its wrinkle resistance and shape retention are very good. After multiple washing and wearing, the clothes can still remain flat and not easily deformed. In view of the advantages of polyester fiber, using polyester fiber to solve the problem of wool fabrics being easy to shrink and deform has great practical significance. Summary of the invention

[0005] In view of the deficiencies in the prior art, an object of the present invention is to provide a flexible high-strength composite fabric and a preparation method thereof.

[0006] In order to achieve the above object, the present invention adopts the following technical scheme:

[0007] A method for preparing a flexible high-strength composite fabric comprises the following steps:

[0008] S1, performing plasma surface treatment on wool fiber and polyester fiber to obtain pretreated wool fiber and pretreated polyester fiber;

[0009] S2, adding dopamine hydrochloride to Tris-HCl buffer, then adding pretreated wool fiber, soaking for 16-24 hours, taking out after soaking, washing with water, and vacuum drying to obtain modified wool fiber;

[0010] S3, dispersing the pretreated polyester fiber in deionized water, then adding epichlorohydrin and guanidine sulfamate thereto, heating and stirring to react, and after the reaction is completed, filtering, washing and drying the reaction product to obtain the modified polyester fiber;

[0011] S4, blending the modified wool fiber and the modified polyester fiber to form warp yarn and weft yarn, and then cross-weaving the warp yarn and the weft yarn to obtain a fabric base cloth;

[0012] S5, padding the fabric base fabric in the finishing liquid, and then baking, washing and drying the padding fabric base fabric to obtain a flexible high-strength composite fabric.

[0013] Specifically, in step S1, the specific process of plasma surface treatment is: after evacuating the plasma instrument, oxygen is introduced, the power is set to 100-200W, and the treatment time is 5-10min.

[0014] More specifically, the power can be selected as 100W, 110W, 120W, 130W, 140W, 150W, 160W, 170W, 180W, 190W, and 200W; the processing time can be selected as 5min, 6min, 7min, 8min, 9min, and 10min; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0015] Specifically, in step S2, the dosage ratio of dopamine hydrochloride, Tris-HCl buffer and pretreated wool fiber is 3-4g:100mL:10-15g, for example, 3g:100mL:10g, 3g:100mL:12g, 3g:100mL:15g, 3.5g:100mL:10g, 3.5g:100mL:15g, 4g:100mL:10g, 4g:100mL:12g, 4g:100mL:15g can be selected, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] More specifically, the concentration of the selected Tris-HCl buffer is 0.1-0.5 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L can be selected, but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0017] Specifically, in step S3, the mass ratio of the pretreated polyester fiber, epichlorohydrin and guanidine sulfamate is 10-20:3-5:4-8, and more preferably 12-16:3-4:5-6.

[0018] Specifically, in step S3, the temperature of the heating and stirring reaction is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C, and 80°C can be selected; the time of the heating and stirring reaction is 2-5h, for example, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, and 5h can be selected; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0019] Specifically, in step S4, the content of modified wool fiber in the warp yarn is 50-60wt%, and the content of modified polyester fiber is 40-50wt%; the content of modified wool fiber in the weft yarn is 70-80wt%, and the content of modified polyester fiber is 20-30wt%.

[0020] Specifically, in step S4, the linear density of the warp yarn is 15-20tex, and the linear density of the weft yarn is 15-20tex; the specific weaving process is: the warp yarn and the weft yarn are interwoven with each other in a plain weave manner, the warp yarn density is 360-365 yarns / 10cm, and the weft yarn density is 325-330 yarns / 10cm.

[0021] Specifically, in step S5, the finishing solution comprises the following components in parts by weight: 100 parts of water, 5-10 parts of carboxymethyl chitosan, 4-8 parts of blocked isocyanate crosslinking agent, 1-2 parts of nano-silicon dioxide, and 0.5-1 part of sodium dodecyl sulfate.

[0022] Specifically, in step S5, the bath ratio of the fabric base fabric and the finishing liquid is 1:10-15, for example, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15 can be selected; but it is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0023] Specifically, in step S5, the padding liquid rate of the fabric base fabric is 70-80%.

[0024] Specifically, in step S5, the baking temperature is 120-150° C., and the baking time is 10-15 minutes.

[0025] The present invention also provides a flexible high-strength composite fabric prepared by the above preparation method.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The present invention forms micropores and slits on the fiber surface by plasma treatment of wool fiber and polyester fiber, providing more physical anchoring points; at the same time, plasma treatment can activate the fiber surface and introduce polar functional groups such as carboxyl and hydroxyl groups, which is beneficial to the subsequent reaction.

[0028] (2) The present invention utilizes dopamine to modify wool fibers and deposits a layer of polydopamine on the surface of the wool fibers. After the wool fibers are modified with polydopamine, amino active functional groups are introduced, which is beneficial to the subsequent reactions. At the same time, polydopamine has excellent flame retardant properties. Introducing it into composite fabrics is beneficial to improving the flame retardant properties of the fabrics.

[0029] (3) In the present invention, guanidine sulfonate is grafted onto polyester fiber through the cross-linking effect of epichlorohydrin. Guanidine sulfonate has excellent antibacterial and flame retardant properties. Its introduction into the composite fabric enhances the antibacterial and flame retardant properties of the fabric.

[0030] (4) The finishing liquid provided by the present invention contains a blocked isocyanate crosslinker, which can coexist stably with active groups (hydroxyl, amino, etc.) for a long time at room temperature. During the baking process, the isocyanate crosslinker releases -NCO groups and undergoes crosslinking reactions with hydroxyl and amino groups, thereby improving the bonding strength between the modified wool fiber and the modified polyester fiber, thereby improving the mechanical strength of the composite fabric. At the same time, carboxymethyl chitosan contains a large number of hydrophilic groups such as hydroxyl groups. Carboxymethyl chitosan adheres to the surface of the composite fabric through chemical crosslinking, making the fabric have good hygroscopicity and soft skin-friendly. In addition, the polyhydroxy structure of carboxymethyl chitosan can form a highly graphitized hybrid carbon layer on the surface of the material when heated. This carbon layer can cut off the heat and oxygen exchange between the material and the external environment, thereby achieving a flame retardant effect. Carboxymethyl chitosan also has a certain antibacterial effect, and works together with aminosulfonic acid guanidine and polydopamine to further improve the flame retardant and antibacterial properties of the composite fabric. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below through specific preferred embodiments, but the present invention is not limited to the following embodiments.

[0032] It should be noted that, unless otherwise specified, the chemical reagents involved in the present invention were purchased through commercial channels.

[0033] The average diameter of the wool fiber used in the embodiment of the present invention is 11-12 μm, the average diameter of the polyester fiber is 10-15 μm, the particle size of the nano-silicon dioxide is 40-60 nm, and the blocked isocyanate cross-linking agent is purchased from Guangzhou Wanjun Chemical Technology Co., Ltd., model C66.

[0034] Example 1

[0035] A method for preparing a flexible high-strength composite fabric comprises the following steps:

[0036] S1. Surface treatment of wool fiber and polyester fiber by plasma. The specific process of the treatment is as follows: after vacuuming the plasma instrument, oxygen is introduced, the power is set to 200 W, and the treatment time is 5 min to obtain pretreated wool fiber and pretreated polyester fiber;

[0037] S2, adding 3 g of dopamine hydrochloride to 100 mL of 0.1 mol / L Tris-HCl buffer, then adding 10 g of pretreated wool fiber, soaking for 16 h, taking out after soaking, washing with water, and vacuum drying to obtain modified wool fiber;

[0038] S3, dispersing 10 g of pretreated polyester fiber in 150 mL of deionized water, then adding 3 g of epichlorohydrin and 4 g of guanidine sulfamate thereto, heating and stirring at 60° C. for 5 h, after the reaction is completed, filtering, washing and drying the reaction product to obtain modified polyester fiber;

[0039] S4, blending the modified wool fiber and the modified polyester fiber to form warp yarn and weft yarn, wherein the content of the modified wool fiber in the warp yarn is 50wt%, and the content of the modified polyester fiber is 50wt%, and the content of the modified wool fiber in the weft yarn is 70wt%, and the content of the modified polyester fiber is 30wt%, and then the warp yarn and the weft yarn are cross-woven to obtain a fabric base cloth, wherein the linear density of the warp yarn is 20tex, and the linear density of the weft yarn is 20tex; the specific weaving process is: the warp yarn and the weft yarn are interwoven one above and one below to form a plain weave, the warp yarn density is 360 yarns / 10cm, and the weft yarn density is 325 yarns / 10cm;

[0040] S5. The fabric base fabric is immersed in a finishing liquid with a bath ratio of 1:10, wherein the finishing liquid comprises the following components in parts by weight: 100 parts of water, 10 parts of carboxymethyl chitosan, 5 parts of blocked isocyanate crosslinking agent, 1 part of nano-silicon dioxide, and 1 part of sodium dodecyl sulfate. The fabric base fabric after the immersion treatment is taken out, and the immersion liquid rate is 70%. The fabric base fabric is then baked at 150°C for 10 minutes, washed with water, and dried at 60°C to obtain a flexible high-strength composite fabric.

[0041] Example 2

[0042] A method for preparing a flexible high-strength composite fabric comprises the following steps:

[0043] S1. Surface treatment of wool fiber and polyester fiber by plasma. The specific process of the treatment is as follows: after vacuuming the plasma instrument, oxygen is introduced, the power is set to 100 W, and the treatment time is 10 min to obtain pretreated wool fiber and pretreated polyester fiber;

[0044] S2, adding 4 g of dopamine hydrochloride to 100 mL of 0.1 mol / L Tris-HCl buffer, then adding 15 g of pretreated wool fiber, soaking for 24 h, taking out after soaking, washing with water, and vacuum drying to obtain modified wool fiber;

[0045] S3, dispersing 20g of pretreated polyester fiber in 150mL of deionized water, then adding 5g of epichlorohydrin and 8g of guanidine sulfamate thereto, heating and stirring at 80°C for 2h, after the reaction is completed, filtering, washing and drying the reaction product to obtain modified polyester fiber;

[0046] S4, blending the modified wool fiber and the modified polyester fiber to form warp yarn and weft yarn, wherein the content of the modified wool fiber in the warp yarn is 60wt%, and the content of the modified polyester fiber is 40wt%, and the content of the modified wool fiber in the weft yarn is 70wt%, and the content of the modified polyester fiber is 30wt%, and then the warp yarn and the weft yarn are cross-woven to obtain a fabric base cloth, wherein the linear density of the warp yarn is 20tex, and the linear density of the weft yarn is 20tex; the specific weaving process is: the warp yarn and the weft yarn are interwoven one above and one below to form a plain weave, the warp yarn density is 360 yarns / 10cm, and the weft yarn density is 325 yarns / 10cm;

[0047] S5. The fabric base fabric is immersed in a finishing liquid with a bath ratio of 1:10, wherein the finishing liquid comprises the following components in parts by weight: 100 parts of water, 10 parts of carboxymethyl chitosan, 8 parts of blocked isocyanate crosslinking agent, 2 parts of nano-silicon dioxide, and 1 part of sodium dodecyl sulfate. The fabric base fabric after the immersion treatment is taken out, and the immersion liquid rate is 80%. The fabric base fabric is then baked at 120°C for 15 minutes, washed with water, and dried at 60°C to obtain a flexible high-strength composite fabric.

[0048] Example 3

[0049] A method for preparing a flexible high-strength composite fabric comprises the following steps:

[0050] S1. Surface treatment of wool fiber and polyester fiber by plasma. The specific process of the treatment is as follows: after vacuuming the plasma instrument, oxygen is introduced, the power is set to 100 W, and the treatment time is 10 min to obtain pretreated wool fiber and pretreated polyester fiber;

[0051] S2, adding 4 g of dopamine hydrochloride to 100 mL of 0.5 mol / L Tris-HCl buffer, then adding 12 g of pretreated wool fiber, soaking for 24 h, taking out after soaking, washing with water, and vacuum drying to obtain modified wool fiber;

[0052] S3, dispersing 15g of pretreated polyester fiber in 150mL of deionized water, then adding 4g of epichlorohydrin and 6g of guanidine sulfamate thereto, heating and stirring at 60°C for 4h, after the reaction is completed, filtering, washing and drying the reaction product to obtain modified polyester fiber;

[0053] S4, blending the modified wool fiber and the modified polyester fiber to form warp yarn and weft yarn, wherein the content of the modified wool fiber in the warp yarn is 60wt%, and the content of the modified polyester fiber is 40wt%, and the content of the modified wool fiber in the weft yarn is 80wt%, and the content of the modified polyester fiber is 20wt%, and then cross-weaving the warp yarn and the weft yarn to obtain a fabric base cloth, wherein the linear density of the warp yarn is 20tex, and the linear density of the weft yarn is 20tex; the specific weaving process is: the warp yarn and the weft yarn are interwoven one above and one below to form a plain weave, the warp yarn density is 360 yarns / 10cm, and the weft yarn density is 325 yarns / 10cm;

[0054] S5. The fabric base fabric is immersed in a finishing liquid with a bath ratio of 1:10, wherein the finishing liquid comprises the following components in parts by weight: 100 parts of water, 5 parts of carboxymethyl chitosan, 5 parts of blocked isocyanate crosslinking agent, 1 part of nano-silicon dioxide, and 1 part of sodium dodecyl sulfate. The fabric base fabric after the immersion treatment is taken out, and the immersion liquid rate is 80%. The fabric base fabric is then baked at 120°C for 15 minutes, washed with water, and dried at 60°C to obtain a flexible high-strength composite fabric.

[0055] Example 4

[0056] A method for preparing a flexible high-strength composite fabric comprises the following steps:

[0057] S1. Surface treatment of wool fiber and polyester fiber by plasma. The specific process of the treatment is as follows: after vacuuming the plasma instrument, oxygen is introduced, the power is set to 150 W, and the treatment time is 8 minutes to obtain pretreated wool fiber and pretreated polyester fiber;

[0058] S2, adding 3.5g dopamine hydrochloride to 100mL, 0.2mol / L Tris-HCl buffer, then adding 10g pretreated wool fiber, soaking for 24h, taking out after soaking, washing with water, and vacuum drying to obtain modified wool fiber;

[0059] S3, dispersing 16 g of pretreated polyester fiber in 150 mL of deionized water, then adding 4 g of epichlorohydrin and 8 g of guanidine sulfamate thereto, heating and stirring at 70° C. for 3 h, after the reaction is completed, filtering, washing and drying the reaction product to obtain modified polyester fiber;

[0060] S4, blending the modified wool fiber and the modified polyester fiber to form warp yarn and weft yarn, wherein the content of the modified wool fiber in the warp yarn is 55wt%, and the content of the modified polyester fiber is 45wt%, and the content of the modified wool fiber in the weft yarn is 75wt%, and the content of the modified polyester fiber is 25wt%, and then cross-weaving the warp yarn and the weft yarn to obtain a fabric base cloth, wherein the linear density of the warp yarn is 20tex, and the linear density of the weft yarn is 20tex; the specific weaving process is: the warp yarn and the weft yarn are interwoven one above and one below to form a plain weave, the warp yarn density is 360 yarns / 10cm, and the weft yarn density is 325 yarns / 10cm;

[0061] S5. The fabric base fabric is immersed in a finishing liquid with a bath ratio of 1:10, wherein the finishing liquid comprises the following components in parts by weight: 100 parts of water, 6 parts of carboxymethyl chitosan, 4 parts of blocked isocyanate crosslinking agent, 1 part of nano-silicon dioxide, and 0.5 parts of sodium dodecyl sulfate. The fabric base fabric after the immersion treatment is taken out, and the immersion liquid rate is 80%. The fabric base fabric is then baked at 120°C for 15 minutes, washed with water, and dried at 60°C to obtain a flexible high-strength composite fabric.

[0062] Comparative Example 1

[0063] A method for preparing a flexible high-strength composite fabric comprises the following steps:

[0064] S1. Surface treatment of wool fiber and polyester fiber by plasma. The specific process of the treatment is as follows: after vacuuming the plasma instrument, oxygen is introduced, the power is set to 200 W, and the treatment time is 5 min to obtain pretreated wool fiber and pretreated polyester fiber;

[0065] S2, dispersing 10 g of pretreated polyester fiber in 150 mL of deionized water, then adding 3 g of epichlorohydrin and 4 g of guanidine sulfamate thereto, heating and stirring at 60° C. for 5 h, after the reaction is completed, filtering, washing and drying the reaction product to obtain modified polyester fiber;

[0066] S3, the pretreated wool fiber and the modified polyester fiber are blended to form warp yarn and weft yarn, wherein the content of the pretreated wool fiber in the warp yarn is 50wt%, and the content of the modified polyester fiber is 50wt%, and the content of the weft yarn is 70wt%, and the content of the modified polyester fiber is 30wt%, and then the warp yarn and the weft yarn are cross-woven to obtain a fabric base cloth, the linear density of the warp yarn is 20tex, and the linear density of the weft yarn is 20tex; the specific weaving process is: the warp yarn and the weft yarn are interwoven one above and one below to form a plain weave, the warp yarn density is 360 yarns / 10cm, and the weft yarn density is 325 yarns / 10cm;

[0067] S4. The fabric base fabric is immersed in a finishing liquid with a bath ratio of 1:10, wherein the finishing liquid comprises the following components in parts by weight: 100 parts of water, 10 parts of carboxymethyl chitosan, 5 parts of blocked isocyanate crosslinking agent, 1 part of nano-silicon dioxide, and 1 part of sodium dodecyl sulfate. The fabric base fabric after the immersion treatment is taken out, and the immersion liquid rate is 70%. The fabric base fabric is then baked at 150°C for 10 minutes, washed with water, and dried at 60°C to obtain a flexible high-strength composite fabric.

[0068] Compared with Example 1, Comparative Example 1 did not perform further modification treatment on the pretreated wool fiber.

[0069] Comparative Example 2

[0070] A method for preparing a flexible high-strength composite fabric comprises the following steps:

[0071] S1. Surface treatment of wool fiber and polyester fiber by plasma. The specific process of the treatment is as follows: after vacuuming the plasma instrument, oxygen is introduced, the power is set to 200 W, and the treatment time is 5 min to obtain pretreated wool fiber and pretreated polyester fiber;

[0072] S2, adding 3 g of dopamine hydrochloride to 100 mL of 0.1 mol / L Tris-HCl buffer, then adding 10 g of pretreated wool fiber, soaking for 16 h, taking out after soaking, washing with water, and vacuum drying to obtain modified wool fiber;

[0073] S3, the modified wool fiber and the pretreated polyester fiber are blended to form warp yarn and weft yarn, wherein the content of the modified wool fiber in the warp yarn is 50wt%, and the content of the pretreated polyester fiber is 50wt%, and the content of the modified wool fiber in the weft yarn is 70wt%, and the content of the pretreated polyester fiber is 30wt%, and then the warp yarn and the weft yarn are cross-woven to obtain a fabric base cloth, wherein the linear density of the warp yarn is 20tex, and the linear density of the weft yarn is 20tex; the specific weaving process is: the warp yarn and the weft yarn are interwoven one above and one below to form a plain weave, the warp yarn density is 360 yarns / 10cm, and the weft yarn density is 325 yarns / 10cm;

[0074] S4. The fabric base fabric is immersed in a finishing liquid with a bath ratio of 1:10, wherein the finishing liquid comprises the following components in parts by weight: 100 parts of water, 10 parts of carboxymethyl chitosan, 5 parts of blocked isocyanate crosslinking agent, 1 part of nano-silicon dioxide, and 1 part of sodium dodecyl sulfate. The fabric base fabric after the immersion treatment is taken out, and the immersion liquid rate is 70%. The fabric base fabric is then baked at 150°C for 10 minutes, washed with water, and dried at 60°C to obtain a flexible high-strength composite fabric.

[0075] Compared with Example 1, Comparative Example 2 did not perform further modification treatment on the pretreated polyester fiber.

[0076] Comparative Example 3

[0077] A method for preparing a flexible high-strength composite fabric comprises the following steps:

[0078] S1. Surface treatment of wool fiber and polyester fiber by plasma. The specific process of the treatment is as follows: after vacuuming the plasma instrument, oxygen is introduced, the power is set to 200 W, and the treatment time is 5 min to obtain pretreated wool fiber and pretreated polyester fiber;

[0079] S2, adding 3 g of dopamine hydrochloride to 100 mL of 0.1 mol / L Tris-HCl buffer, then adding 10 g of pretreated wool fiber, soaking for 16 h, taking out after soaking, washing with water, and vacuum drying to obtain modified wool fiber;

[0080] S3, dispersing 10 g of pretreated polyester fiber in 150 mL of deionized water, then adding 3 g of epichlorohydrin and 4 g of guanidine sulfamate thereto, heating and stirring at 60° C. for 5 h, after the reaction is completed, filtering, washing and drying the reaction product to obtain modified polyester fiber;

[0081] S4. Modified wool fiber and modified polyester fiber are blended to form warp yarn and weft yarn, wherein the content of modified wool fiber in the warp yarn is 50wt%, and the content of modified polyester fiber is 50wt%, and the content of modified wool fiber in the weft yarn is 70wt%, and the content of modified polyester fiber is 30wt%. Then the warp yarn and the weft yarn are cross-woven to obtain the fabric, wherein the linear density of the warp yarn is 20tex, and the linear density of the weft yarn is 20tex. The specific weaving process is as follows: the warp yarn and the weft yarn are interwoven with each other in a plain weave manner, wherein the warp yarn density is 360 yarns / 10cm, and the weft yarn density is 325 yarns / 10cm.

[0082] Compared with Example 1, in Comparative Example 3, the fabric was not subjected to padding treatment in the finishing liquid.

[0083] The composite fabrics prepared in Examples 1-4 and Comparative Examples 1-3 were subjected to performance tests, as follows:

[0084] Breaking strength: tested in accordance with GB / T 3923.1-2013 standard;

[0085] Stiffness: Tested in accordance with GB / T 8318.1-2009, the smaller the stiffness value, the softer the fabric;

[0086] Limiting oxygen index: tested in accordance with GB / T 5454-1997 standard;

[0087] Antibacterial performance test: The test was conducted in accordance with GB / T 20944.3-2008 “Evaluation of antibacterial properties of textiles Part 3: Oscillation method”, and the bacteria species was Escherichia coli.

[0088] The test was conducted 3 times and the results were averaged;

[0089] The test results are shown in the following table:

[0090]

[0091] Finally, it should be noted that the above embodiments do not limit the present invention in any form. For those skilled in the art, some modifications and improvements can be made to the present invention. Therefore, any modification or improvement made without departing from the spirit of the present invention belongs to the scope of protection claimed in the present invention.

Claims

1. A method for preparing a flexible high-strength composite fabric, characterized in that: The steps include: S1, performing plasma surface treatment on wool fiber and polyester fiber to obtain pretreated wool fiber and pretreated polyester fiber; S2, adding dopamine hydrochloride to Tris-HCl buffer, then adding pretreated wool fiber, soaking for 16-24 hours, taking out after soaking, washing with water, and vacuum drying to obtain modified wool fiber; S3, dispersing the pretreated polyester fiber in deionized water, then adding epichlorohydrin and guanidine sulfamate thereto, heating and stirring to react, and after the reaction is completed, filtering, washing and drying the reaction product to obtain the modified polyester fiber; S4, blending the modified wool fiber and the modified polyester fiber to form warp yarn and weft yarn, and then cross-weaving the warp yarn and the weft yarn to obtain a fabric base cloth; S5, padding the fabric base fabric in the finishing liquid, and then baking, washing, and drying the padding fabric base fabric to obtain a flexible high-strength composite fabric; Wherein, in step S5, the finishing liquid comprises the following components in parts by weight: 100 parts of water, 5-10 parts of carboxymethyl chitosan, 4-8 parts of blocked isocyanate crosslinking agent, 1-2 parts of nano-silicon dioxide, and 0.5-1 part of sodium dodecyl sulfate.

2. The preparation method according to claim 1, characterized in that: In step S1, the specific process of plasma surface treatment is: after evacuating the plasma instrument, oxygen is introduced, the power is set to 100-200W, and the treatment time is 5-10min.

3. The preparation method according to claim 1, characterized in that: In step S2, the usage ratio of dopamine hydrochloride, Tris-HCl buffer and pretreated wool fiber is 3-4 g:100 mL:10-15 g, and the concentration of Tris-HCl buffer is 0.1-0.5 mol / L.

4. The preparation method according to claim 1, characterized in that: In step S3, the mass ratio of the pretreated polyester fiber, epichlorohydrin and guanidine sulfamate is 10-20:3-5:4-8.

5. The preparation method according to claim 1, characterized in that: In step S3, the temperature of the heating and stirring reaction is 60-80° C., and the time of the heating and stirring reaction is 2-5 h.

6. The preparation method according to claim 1, characterized in that: In step S4, the content of modified wool fiber in the warp yarn is 50-60wt%, and the content of modified polyester fiber is 40-50wt%; the content of modified wool fiber in the weft yarn is 70-80wt%, and the content of modified polyester fiber is 20-30wt%.

7. The preparation method according to claim 1, characterized in that: In step S4, the linear density of the warp yarn is 15-20tex, and the linear density of the weft yarn is 15-20tex; the specific weaving process is: the warp yarn and the weft yarn are interwoven one above and one below to form a plain weave, the warp yarn density is 360-365 yarns / 10cm, and the weft yarn density is 325-330 yarns / 10cm.

8. The preparation method according to claim 1, characterized in that: In step S5, the padding liquid rate of the fabric base fabric is 70-80%.

9. The flexible high-strength composite fabric prepared by the preparation method according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Antibacterial and breathable home textile fabric and making method thereof

    CN108570761A

  • Antibacterial and anti-wrinkle fabric for suit and preparation process thereof

    CN111349995A

  • Antibacterial and hemostatic multifunctional composite hydrogel dressing and preparation method thereof

    CN111388748A

  • Flame-retardant antibacterial fabric and preparation method thereof

    CN111979776A

  • Medical antibacterial spinning fabric and preparation method thereof

    CN114318876A