A method for preparing an inductor by integrated injection molding of a composite magnetic fluid and the prepared inductor

Through the high permeability composite magnetic fluid integrated injection molding process, the problems of coil insulation damage and magnet cracking during hot press molding are solved, and the stability and flexibility of the inductor are achieved. It is suitable for precision electronics and other fields, simplifying the process and Reduced costs.

CN118507243BActive Publication Date: 2024-10-11ZHUZHOU HONGDA MAG-ELECTRIC TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410941991.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-11
Estimated Expiration
2044-07-15

AI Technical Summary

Technical Problem

In the existing hot press molding process, problems such as coil insulation damage, magnet cracking and single mold shape are difficult to meet the needs of high-reliability inductors, especially in the fields of precision electronics, automotive electronics and communication technology.

Method used

The high permeability composite magnetic fluid integrated injection molding process is used to prepare the composite magnetic fluid by mixing ferrite powder with a binder and dispersant, and then coat the inductor coil through injection molding technology at low temperature to form a stable and tight The inductor structure avoids coil varnish cracking and magnet cracking while allowing shape flexibility.

Benefits of technology

It improves the stability and reliability of the inductor, is suitable for high-demand fields, simplifies the process flow, reduces production costs, and achieves optimization of inductor performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118507243B_ABST
    Figure CN118507243B_ABST
Patent Text Reader

Abstract

The present application relates to the field of electronic component manufacturing, and specifically discloses a method for preparing an inductor by integrated composite magnetic fluid injection molding and the prepared inductor. The preparation method comprises the following steps: S1, preparing a high magnetic permeability composite magnetic fluid: mixing ferrite powder with a binder and a dispersant to prepare a composite magnetic fluid, and then grinding and removing impurities; S2, cleaning and drying an inductor coil wound by a high-conductivity metal wire; S3, placing the inductor coil in step S2 in an injection mold, and then injecting the composite magnetic fluid after impurities removal in step S1 into the mold by injection molding to prepare an inductor; the present application also discloses an inductor prepared by the above method, and the present application has the effect of solving the problems of paint film rupture, magnet cracking and mold replacement caused by current hot pressing molding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electronic component manufacturing, and more specifically, to a method for preparing an inductor by integrated composite magnetic fluid injection molding and the prepared inductor. Background Art

[0002] With the development of science and technology, the performance requirements for inductor components are getting higher and higher, especially in the fields of precision electronics, automotive electronics, communication technology, etc. The existing one-piece molded inductor molding process is to use ferrite alloy powder and coils through a hot pressing process to form an integrated structure. The specific operation of hot pressing molding is to place the wound coil in the hot press mold, and then hot press the ferrite powder on the coil to obtain an one-piece molded inductor through hot pressing molding. However, this method has the following disadvantages: 1) Coil insulation damage problem: During hot pressing molding, ferrite magnetic powder applies high pressure to the coil, causing the paint film to rupture and damage the insulation of the coil; 2) Magnet cracking: The internal cracks of the powder one-piece molded inductor usually appear around the coil and the center column of the product, resulting in characteristic failure, abnormal inductor sound and product cracking failure; 3) Hot pressing molding is based on the shape of the mold, and the shape is single. When the shape needs to be changed, the mold needs to be replaced.

[0003] In order to solve the defects of existing materials and processes and meet the demand for high-reliability inductive devices in the fields of precision electronics, automotive electronics, and communication technology, it is necessary to provide a new one-piece molding process to solve the above problems. Summary of the invention

[0004] In order to solve the problems of paint film rupture, magnet cracking and mold replacement caused by current hot pressing molding, the present application provides a method for preparing an inductor using high magnetic permeability composite magnetic fluid integrated injection molding and the prepared inductor.

[0005] In a first aspect, the present application provides a method for preparing an inductor by integrated composite magnetic fluid injection molding, which adopts the following technical solution:

[0006] A method for preparing an inductor by integrated composite magnetic fluid injection molding comprises the following steps:

[0007] S1. Preparation of high magnetic permeability composite magnetic fluid: mixing ferrite powder with a binder and a dispersant to obtain a composite magnetic fluid, and then grinding and removing impurities;

[0008] S2, cleaning and drying the inductor coil wound by the high-conductivity metal wire;

[0009] S3, placing the inductor coil in step S2 in an injection mold, and then injecting the composite magnetic fluid after the impurities are removed in step S1 into the mold by injection molding to obtain an inductor.

[0010] By adopting the above technical scheme, the ferrite powder is mixed with a binder and a dispersant in the present application to ensure the magnetic properties and formability of the composite magnetic fluid, and then the particles in the composite magnetic fluid are ball milled to achieve a dispersion effect and particle size adjustment, and then the impurities are removed to improve the purity and stability of the magnetic fluid; in addition, the inductor coil is cleaned to remove oil and impurities on the surface of the coil, and then dried to prevent moisture from affecting the insulating layer, and then the composite magnetic fluid is injected into the mold to coat the coil, which can ensure that the magnetic fluid is evenly and tightly wrapped around the coil, thereby effectively avoiding the cracking of the magnet, ensuring the stability and consistency of the inductor, and also solving the problem of coil paint film rupture caused by high pressure in the traditional hot pressing process, improving the reliability and durability of the product, and finally obtaining an inductor with excellent inductance performance and stability, which is suitable for high-demand fields such as precision electronics, automotive electronics and communication technology. In addition, the injection molding process provided in the present application can form inductors of any shape and special shape, which increases the flexibility of the design, and simplifies the preparation process, improves production efficiency, and reduces production costs.

[0011] Optionally, in the composite magnetic fluid raw material, the added amount of each raw material is as follows: 91-95 parts of ferrite powder, 4-6 parts of binder, and 1-3 parts of dispersant.

[0012] By adopting the above technical solution, when the composite magnetic fluid is prepared in the above proportion, especially by controlling the amount of binder added, the composite magnetic fluid has excellent fluidity, thereby realizing the injection molding process.

[0013] Optionally, the binder is paraffin.

[0014] By adopting the above technical solution, when paraffin wax is used as the binder, the paraffin wax has a low melting point and can be melted at a lower temperature, thereby achieving bonding flow to the ferrite powder and realizing injection molding. Moreover, the temperature of the molten paraffin wax is low, and the coil protective film will not melt during injection molding.

[0015] Optionally, the dispersant is selected from one or more of fatty alcohol polyoxyethylene ether, lignin sulfonate, and p-methoxy fatty amide benzene sulfonic acid.

[0016] By adopting the above technical solution, the selection of the above dispersant is more helpful to improve the dispersion uniformity of paraffin and ferrite powder, and is helpful to improve the magnetic permeability performance of the composite magnetic fluid.

[0017] Optionally, the binder comprises paraffin and magnetic polymer microcapsules in a mass ratio of 1:(0.4-0.6), wherein the magnetic polymer microcapsules comprise a core material, an inner coating layer and an outer coating layer arranged in sequence from the inside to the outside, the core material comprises a ferricyanide complex and a nickel-iron composite powder, the inner coating layer wall material comprises vinyl ferrocene-acrylate polymer, and the outer coating layer wall material comprises COPNA resin and polyamide resin.

[0018] By adopting the above technical solution, when paraffin is used as the binder, since paraffin as a non-magnetic material will dilute the magnetic components of ferrite powder, the concentration of magnetic substances in the overall mixture will be reduced, thereby reducing the overall magnetic permeability; in addition, the interface effect existing at the interface between paraffin and ferrite powder will hinder the propagation of the magnetic field and the arrangement of magnetic moments, thereby reducing the overall magnetic permeability. In addition, during the mixing process, the particles of ferrite powder are separated by paraffin, resulting in an increase in the distance between the particles, affecting the interaction between the magnetic moments, thereby reducing the magnetic permeability.

[0019] Therefore, paraffin wax and magnetic polymer microcapsules are selected as the binder in the present application, so that the bonding and melting fluidity of paraffin wax can be utilized to realize the injection molding of the composite magnetic fluid, and the polymer microcapsule coating material is a polymer obtained by copolymerization of polyamide resin and acrylic acid monomer, which can further improve the fluidity of paraffin wax, make the solid solution concentration of paraffin wax finer, thereby improving its fluidity. The composite magnetic fluid finally obtained has better fluidity and is more conducive to injection molding.

[0020] Moreover, the magnetic polymer microcapsules can also form a melt to realize the injection molding of the composite magnetic fluid, and the nickel of the nickel-iron composite powder in the core material of the magnetic polymer microcapsules can form a complex with the carbon-carbon double bond in the vinyl ferrocene polymer, and then combined with the vinyl ferrocene polymer, the prepared polymer microcapsules exhibit certain magnetism, and then combined with the magnetism of the ferric cyanide complex, the magnetic polymer microcapsules are melted to form a fluid to realize the injection molding of the composite magnetic fluid. When the polyamide is melted, the above-mentioned iron and nickel form a chemical complex with the above-mentioned high molecular polymer and flow accordingly, forming a magnetic conduction effect between the dispersed ferrite powder particles. Finally, it is found that the addition of the magnetic polymer microcapsules makes the composite magnetic fluid not only have excellent fluidity, realize injection molding, but also have excellent magnetic permeability performance, and the inductance performance of the final inductor is better.

[0021] Optionally, the vinyl ferrocene-acrylate polymer is prepared by the following method:

[0022] 1) Add vinyl ferrocene, methyl methacrylate, acrylamide, maleic anhydride and initiator into tetrahydrofuran, stir and mix to prepare a monomer mixture;

[0023] 2) Add stabilizer and ethylene glycol dimethacrylate to the monomer mixture, and then react at 80-90° C. for 2-3 hours, then stop heating, cool to room temperature, centrifuge, and wash with water to obtain vinyl ferrocene-acrylate polymer.

[0024] By adopting the above technical scheme, vinyl ferrocene monomer and acrylate monomer are first added to tetrahydrofuran, and then under the action of an initiator, vinyl ferrocene is polymerized with vinyl monomers such as methyl methacrylate and acrylamide to form a polymer main chain. The maleic anhydride monomer contains two unsaturated double bonds, which are grafted on the polymer main chain through polymerization with methyl methacrylate, so that the final vinyl ferrocene-acrylate polymer contains unsaturated double bonds, which can form a complex with the nickel-iron composite powder to achieve the introduction of magnetic particles on the polymer. In addition, since the acrylate polymer also has the characteristics of low melting point viscosity, the polymer is also helpful for injection molding of ferrite powder, while improving the magnetic conductivity of the composite magnetic fluid.

[0025] Optionally, when preparing the vinyl ferrocene-acrylate polymer, the raw materials are added according to the following weight parts: 10-20 parts of tetrahydrofuran, 15-25 parts of vinyl ferrocene, 15-25 parts of methyl methacrylate, 10-15 parts of acrylamide, 15-20 parts of maleic anhydride, 1-3 parts of initiator, 1-3 parts of stabilizer and 3-5 parts of ethylene glycol dimethacrylate.

[0026] By adopting the above technical solution and controlling the above raw materials, especially the amount of each monomer added, a polymer with a special macromolecular structure is finally obtained, which has better fluidity and higher magnetic permeability, and better overall performance.

[0027] Optionally, the ferric cyanide complex is prepared by the following method:

[0028] Dissolving ferric chloride in water to prepare a ferric chloride solution with a mass concentration of 35-45%;

[0029] Dissolving sodium cyanide in water to prepare a sodium cyanide solution with a mass concentration of 25-35%;

[0030] Then, the sodium cyanide solution is poured into the ferric chloride solution and reacted for 40-60 minutes, then filtered and washed with water to obtain the ferric cyanide complex.

[0031] By adopting the above technical solution and performing the above operation, the trivalent iron ions and the cyanide ions react to form a ferric cyanide complex with certain magnetism, which is then used as a core material and a polymer to form a magnetic polymer microcapsule.

[0032] Optionally, the magnetic polymer microcapsules are prepared by the following method:

[0033] The ferric cyanide complex and nickel-iron composite powder are mixed and granulated to obtain core material particles, and then the vinyl ferrocene-acrylate polymer is dissolved in ethanol and sprayed on the surface of the core material as an inner coating solution, and dried to form an inner coating layer, and then COPNA resin and polyamide resin are dissolved in ethanol and sprayed on the inner coating layer as an outer coating solution, and dried to obtain magnetic polymer microcapsules.

[0034] Optionally, the mass ratio of the ferric cyanide complex to the nickel-iron composite powder is 1:(1.5-1.8), and the mass ratio of the COPNA resin to the polyamide resin is 1:(2-3);

[0035] The added mass ratio of the core material particles to the inner coating layer solution is 1:(1.5-2), and the added mass ratio of the core material particles to the outer coating layer solution is 1:(1.2-1.5).

[0036] By adopting the above technical solution and selecting the above addition ratio, the composite magnetic fluid finally obtained has better comprehensive performance.

[0037] Optionally, 1-3 parts by weight of aromatic aldehyde are further added to the composite magnetic fluid.

[0038] By adopting the above technical solution, it may be because the aromatic aldehyde and COPNA resin also obtain magnetism through chemical reaction in the presence of magnetism. When a small amount of aromatic aldehyde is added to the composite magnetic fluid, the magnetic permeability of the composite magnetic fluid is better, and the performance of the final inductor is better.

[0039] In a second aspect, the present application provides an inductor, which adopts the following technical solution:

[0040] An inductor is prepared by the preparation method as described above.

[0041] By adopting the above technical scheme, the method for preparing the inductor by the method provided in the present application is simpler and more convenient, and avoids the cracking of the magnet, ensuring the stability and consistency of the inductor, and also solves the problem of coil paint film rupture caused by high pressure in the traditional hot pressing process, thereby improving the reliability and durability of the product. The final inductor has excellent inductance performance and stability, and is suitable for high-demand fields such as precision electronics, automotive electronics and communication technology.

[0042] In summary, this application has the following beneficial effects:

[0043] 1. In the present application, ferrite powder is mixed with a binder and a dispersant to ensure the magnetic properties and formability of the composite magnetic fluid. Then, the composite magnetic fluid is injected into the mold to cover the coil, which can ensure that the magnetic fluid is evenly and tightly wrapped around the coil, thereby effectively avoiding the cracking of the magnet and ensuring the stability and consistency of the inductor. It also solves the problem of coil paint film rupture caused by high pressure in the traditional hot pressing process, improves the reliability and durability of the product, and finally obtains an inductor with excellent inductance performance and stability, which is suitable for high-demand fields such as precision electronics, automotive electronics and communication technology; in addition, the injection molding process provided in the present application can form inductors of any shape and special shape, which increases the flexibility of design, and simplifies the preparation process, improves production efficiency, and reduces production costs;

[0044] 2. When paraffin wax is used as the binder in the present application, the paraffin wax has a low melting point and can be melted at a relatively low temperature, thereby achieving bonding and flow of the ferrite powder and realizing injection molding. Moreover, the temperature of the molten paraffin wax is relatively low, and the coil protective film will not melt during injection molding.

[0045] 3. In the present application, paraffin wax and magnetic polymer microcapsules are selected as the binder, and the microcapsule coating material is a polymer obtained by copolymerizing polyamide resin and acrylic acid monomer, which can form a melt to realize the injection molding of the composite magnetic fluid. Moreover, the nickel of the nickel-iron composite powder in the core material of the magnetic polymer microcapsule can form a complex with the carbon-carbon double bond in the vinylated ferrocene polymer, and then combined with the vinylated ferrocene polymer, the prepared polymer microcapsules exhibit certain magnetism, and then combined with the magnetism of the ferric cyanide complex, the magnetic polymer microcapsules are melted to form a fluid to realize the injection molding of the composite magnetic fluid. When the polyamide is melted, the above-mentioned iron and nickel form a chemical complex with the above-mentioned high molecular polymer and flow accordingly, forming a magnetic conduction effect between the dispersed ferrite powder particles. Finally, it is found that the addition of magnetic polymer microcapsules makes the composite magnetic fluid not only have excellent fluidity, realizing injection molding, but also have excellent magnetic permeability performance, and the inductance performance of the final inductor is better. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 is a cross-sectional view of the inductor obtained in Example 1 of the present application;

[0047] Figure 2 is a schematic diagram of the inductor coil structure of the inductor of Example 1 of the present application;

[0048] In the figure, 1. inductor; 2. casing. DETAILED DESCRIPTION

[0049] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0050] In the following examples, the COPNA resin is an aromatic resin (also known as condensed polycyclic polynuclear aromatic hydrocarbon (COPNA) resin) of the model FJSZ produced by Wuhan Baohua Petrochemical New Materials Development Co., Ltd.; the acrylic resin is an acrylic resin of the model RESINHF-05A produced by Dow Chemical;

[0051] The ferrite powder in the following embodiments is manganese-zinc ferrite magnetic powder provided by Qinghe County Dongjun Metal Materials Co., Ltd.

[0052] The following preparation example is an example of the preparation of magnetic polymer microcapsules

[0053] Preparation Example 1

[0054] A method for preparing magnetic polymer microcapsules comprises the following steps:

[0055] Step 1: Prepare the core material:

[0056] Dissolving ferric chloride in water to prepare a ferric chloride solution with a mass concentration of 40%, dissolving sodium cyanide in water to prepare a sodium cyanide solution with a mass concentration of 30%, then pouring the sodium cyanide solution into the ferric chloride solution, reacting for 50 minutes, filtering, and washing with water to prepare a ferric cyanide complex;

[0057] The ferric cyanide complex and nickel 50 iron 50 composite powder (made by mixing nickel powder and iron powder in a mass ratio of 1:1 and sintering) were mixed in a mass ratio of 1:1.6 and granulated to obtain core material particles;

[0058] Step 2: Preparation of vinyl ferrocene-acrylate polymer: The specific operation is as follows:

[0059] 1) Add 20 g of vinyl ferrocene, 20 g of methyl methacrylate, 12 g of acrylamide, 18 g of maleic anhydride and 2 g of initiator benzoyl peroxide to 15 g of tetrahydrofuran, stir and mix to prepare a monomer mixture;

[0060] 2) Add 2g of stabilizer polyethylene glycol 700 and 4g of ethylene glycol dimethacrylate to the monomer mixture, and then react at 85°C for 2.5h, stop heating, cool to room temperature, centrifuge, and wash with water to obtain vinyl ferrocene-acrylate polymer;

[0061] Step 3: Coating: The vinyl ferrocene-acrylate polymer obtained in step 2 is dissolved in 2 times the mass of ethanol and then sprayed on the surface of the core material as an inner coating solution, and then dried to form an inner coating layer. Then, COPNA resin and polyamide resin are mixed and dissolved in 2 times the mass of ethanol, and then sprayed on the inner coating layer as an outer coating solution, and then dried to obtain magnetic polymer microcapsules;

[0062] Among them, in step three, the added mass ratio of COPNA resin and polyamide resin is 1:2.5, the added mass ratio of core material particles and inner coating layer solution is 1:1.8, and the added mass ratio of core material particles and outer coating layer solution is 1:1.3.

[0063] Preparation Example 2

[0064] A method for preparing magnetic polymer microcapsules comprises the following steps:

[0065] Step 1: Prepare the core material:

[0066] The ferric chloride is dissolved in water to prepare a ferric chloride solution with a mass concentration of 35%, and the sodium cyanide is dissolved in water to prepare a sodium cyanide solution with a mass concentration of 25%, and then the sodium cyanide solution is poured into the ferric chloride solution to react for 40 minutes, filtered, and washed with water to prepare a ferric cyanide complex;

[0067] The ferric cyanide complex and nickel 50 iron 50 composite powder (made by mixing nickel powder and iron powder in a mass ratio of 1:1 and sintering) were mixed in a mass ratio of 1:1.5 and granulated to obtain core material particles;

[0068] Step 2: Preparation of vinyl ferrocene-acrylate polymer: The specific operation is as follows:

[0069] 1) Add 15 g of vinyl ferrocene, 15 g of methyl methacrylate, 10 g of acrylamide, 15 g of maleic anhydride and 1 g of initiator benzoyl peroxide to 10 g of tetrahydrofuran, stir and mix to prepare a monomer mixture;

[0070] 2) Add 1g of stabilizer polyethylene glycol 700 and 3g of ethylene glycol dimethacrylate to the monomer mixture, then react at 80°C for 3h, stop heating, cool to room temperature, centrifuge, and wash with water to obtain vinyl ferrocene-acrylate polymer; Step 3: Coating: dissolve the vinyl ferrocene-acrylate polymer obtained in step 2 in 2 times the mass of ethanol and spray it on the surface of the core material as an inner coating solution, dry to form an inner coating layer, then mix COPNA resin and polyamide resin, dissolve them in 2 times the mass of ethanol of the mixture and spray them on the inner coating layer as an outer coating solution, dry to obtain magnetic polymer microcapsules;

[0071] Among them, in step three, the added mass ratio of COPNA resin and polyamide resin is 1:2, the added mass ratio of core material particles and inner coating layer solution is 1:1.5, and the added mass ratio of core material particles and outer coating layer solution is 1:1.2.

[0072] Preparation Example 3

[0073] A method for preparing magnetic polymer microcapsules comprises the following steps:

[0074] Step 1: Prepare the core material:

[0075] The ferric chloride is dissolved in water to prepare a ferric chloride solution with a mass concentration of 45%, and the sodium cyanide is dissolved in water to prepare a sodium cyanide solution with a mass concentration of 35%, and then the sodium cyanide solution is poured into the ferric chloride solution to react for 60 minutes, filtered, and washed with water to prepare a ferric cyanide complex;

[0076] The ferric cyanide complex and nickel 50 iron 50 composite powder (made by mixing nickel powder and iron powder in a mass ratio of 1:1 and sintering) were mixed in a mass ratio of 1:1.8 and granulated to obtain core material particles;

[0077] Step 2: Preparation of vinyl ferrocene-acrylate polymer: The specific operation is as follows:

[0078] 1) Add 25 g of vinyl ferrocene, 25 g of methyl methacrylate, 15 g of acrylamide, 20 g of maleic anhydride and 3 g of initiator benzoyl peroxide to 20 g of tetrahydrofuran, stir and mix to obtain a monomer mixture;

[0079] 2) Add 3g of stabilizer polyethylene glycol 700 and 5g of ethylene glycol dimethacrylate to the monomer mixture, then react at 90°C for 2h, stop heating, cool to room temperature, centrifuge, and wash with water to obtain vinyl ferrocene-acrylate polymer; Step 3: Coating: dissolve the vinyl ferrocene-acrylate polymer obtained in step 2 in 2 times the mass of ethanol and spray it on the surface of the core material as an inner coating solution, dry to form an inner coating layer, then mix COPNA resin and polyamide resin, dissolve them in 2 times the mass of the mixture of ethanol and spray them on the inner coating layer as an outer coating solution, dry to obtain magnetic polymer microcapsules;

[0080] Among them, in step three, the added mass ratio of COPNA resin and polyamide resin is 1:3, the added mass ratio of core material particles and inner coating layer solution is 1:2, and the added mass ratio of core material particles and outer coating layer solution is 1:1.5.

[0081] Preparation Example 4

[0082] A method for preparing magnetic polymer microcapsules is carried out according to the method in Preparation Example 1, except that maleic anhydride is not added when preparing the vinyl ferrocene-acrylate polymer in step 2.

[0083] Preparation Example 5

[0084] A method for preparing magnetic polymer microcapsules is carried out according to the method in Preparation Example 1, except that no ferric cyanide complex is added to the core material.

[0085] Preparation Example 6

[0086] A method for preparing magnetic polymer microcapsules is carried out according to the method in Preparation Example 1, except that no inner coating layer is applied, and COPNA resin and polyamide resin are directly coated on the core particles prepared in step 1 to form an outer coating layer.

[0087] Preparation Example 7

[0088] A method for preparing magnetic polymer microcapsules is carried out according to the method in Preparation Example 1, except that an equal amount of COPNA resin in the outer coating layer is replaced by polyamide resin.

[0089] Preparation Example 8

[0090] A method for preparing magnetic polymer microcapsules is carried out according to the method in Preparation Example 1, except that the inner coating layer wall material vinyl ferrocene-acrylate polymer is replaced by an equal amount of acrylic resin.

[0091] Example 1

[0092] A method for preparing an inductor by integral injection molding of a composite magnetic fluid, referring to Figure 1 and Figure 2 , including the following steps:

[0093] S1. Preparation of high magnetic permeability composite magnetic fluid: 93.4 g of ferrite powder, 5.5 g of binder and 1.1 g of dispersant were mixed to obtain a composite magnetic fluid, and then the composite magnetic fluid was ground using a ball mill, and then filtered and degassed to remove impurities and bubbles;

[0094] S2. Reference Figure 2 , cleaning and drying the inductor coil 1 wound by the high-conductivity metal wire, ensuring that there is no impurity on the surface of the inductor coil 1;

[0095] S3, placing the inductor coil 1 in step S2 in an injection mold, then loading the composite magnetic fluid in step S1 into the barrel of an injection molding machine, and then starting the injection molding machine to inject the composite magnetic fluid into the mold to cover the coil, and the magnetic fluid is cooled and solidified to form Figure 1 Middle shell 2, demoulding, obtain as Figure 1 The one-piece molded inductor shown.

[0096] The binder in step S1 is paraffin wax and the magnetic polymer microcapsules prepared in Preparation Example 1 in a mass ratio of 1:0.5, and the dispersant is AEO-9.

[0097] Example 2

[0098] A method for preparing an inductor by integrated composite magnetic fluid injection molding comprises the following steps:

[0099] S1. Preparation of high magnetic permeability composite magnetic fluid: 91 g of ferrite powder, 6 g of binder and 3 g of dispersant were mixed to obtain a composite magnetic fluid, and then the composite magnetic fluid was ground using a ball mill, and then filtered and degassed to remove impurities and bubbles;

[0100] S2. Clean and dry the inductor coil wound by the highly conductive metal wire to ensure that there is no impurity on the surface of the inductor coil;

[0101] S3, placing the inductor coil in step S2 in an injection mold, then loading the composite magnetic fluid in step S1 into the barrel of an injection molding machine, then starting the injection molding machine, injecting the composite magnetic fluid into the mold to cover the coil, and forming a shell after the magnetic fluid is cooled and solidified, and demolding to obtain an integrally formed inductor.

[0102] The binder in step S1 is paraffin wax and the magnetic polymer microcapsules prepared in Preparation Example 2 in a mass ratio of 1:0.4, and the dispersant is sodium lignin sulfonate.

[0103] Example 3

[0104] A method for preparing an inductor by integrated composite magnetic fluid injection molding comprises the following steps:

[0105] S1. Preparation of high magnetic permeability composite magnetic fluid: 95 g of ferrite powder, 4 g of binder and 1 g of dispersant were mixed to obtain a composite magnetic fluid, and then the composite magnetic fluid was ground using a ball mill, and then filtered and degassed to remove impurities and bubbles;

[0106] S2. Clean and dry the inductor coil wound by the highly conductive metal wire to ensure that there is no impurity on the surface of the inductor coil;

[0107] S3, placing the inductor coil in step S2 in an injection mold, then loading the composite magnetic fluid in step S1 into the barrel of an injection molding machine, then starting the injection molding machine, injecting the composite magnetic fluid into the mold to cover the coil, and forming a shell after the magnetic fluid is cooled and solidified, and demolding to obtain an integrally formed inductor.

[0108] The binder in step S1 is paraffin wax and the magnetic polymer microcapsules prepared in Preparation Example 3 in a mass ratio of 1:0.6, and the dispersant is one or more of fatty alcohol polyoxyethylene ether, lignin sulfonate, and p-methoxy fatty amide benzene sulfonic acid.

[0109] Embodiment 4-8

[0110] A method for preparing an inductor by composite magnetic fluid integral injection molding is carried out according to the method in Example 1, except that the magnetic polymer microcapsules in step S1 are respectively selected from the magnetic polymer microcapsules prepared in Preparation Examples 4-8.

[0111] Example 9

[0112] A method for preparing an inductor by integrated composite magnetic fluid injection molding is carried out according to the method in Example 1, except that paraffin is used as the binder in step S1.

[0113] Example 10

[0114] A method for preparing an inductor by integral injection molding of a composite magnetic fluid is carried out according to the method in Example 1, except that 2g of aromatic aldehyde is also added to the composite magnetic fluid.

[0115] Embodiment 11

[0116] A method for preparing an inductor by integral injection molding of a composite magnetic fluid is carried out according to the method in Example 1, except that 1g of aromatic aldehyde is further added to the composite magnetic fluid.

[0117] Example 12

[0118] A method for preparing an inductor by integral injection molding of a composite magnetic fluid is carried out according to the method in Example 1, except that 3g of aromatic aldehyde is also added to the composite magnetic fluid.

[0119] Comparative Example 1

[0120] A method for preparing an inductor by integrated composite magnetic fluid injection molding is carried out according to the method in Example 1, except that in step S1, the amount of binder added is 3 g, the amount of ferrite powder added is 95.9 g, and the amount of dispersant added is 1.1 g.

[0121] Comparative Example 2

[0122] A method for preparing an inductor by integrated composite magnetic fluid injection molding is carried out according to the method in Example 1, except that in step S1, the amount of binder added is 7g, the amount of ferrite powder added is 91.9g, and the amount of dispersant added is 1.1g.

[0123] Performance Testing

[0124] First, the flow lengths of the composite magnetic fluids prepared in the above embodiments and comparative examples were tested and counted, and the test results are shown in Table 1 below.

[0125] Table 1:

[0126]

[0127] The paint film and magnet of the inductor obtained by the one-piece injection molding provided in the embodiment of the present application did not show any cracking phenomenon. In addition, the initial magnetic permeability of the shell formed after the magnetic fluid in the embodiment of the present application and the comparative example was tested, and the initial inductance L@0A (μH) of the obtained inductor was tested. The test results are shown in Table 2 below.

[0128] Table 2:

[0129]

[0130] Combined with the data in Table 1 and Table 2 above, the composite magnetic fluid prepared in the embodiment of the present application has excellent fluidity and higher magnetic permeability, and the inductor prepared therefrom has better inductance performance. Combined with the test results of Example 1 and Example 4, it can be seen that when maleic anhydride is not added to the magnetic polymer microcapsule in Example 4, its magnetic permeability is reduced. Since maleic anhydride and acrylate monomers are polymerized to introduce carbon-carbon unsaturated functional groups, it is convenient for nickel-iron composite powder to form chemical complexation with the wall material, which is more conducive to the conduction of the magnetic material after subsequent injection molding and melting. In addition, in Example 5, no ferric cyanide complex is added to the core material, and its magnetic permeability performance decreases significantly, while the fluidity does not change much. The addition of the above substances will not cause loss of fluidity while improving the magnetic permeability performance. Combined with the test results in Example 1 and Example 6, when no vinyl ferrocene-acrylate polymer was added as the inner coating layer in Example 6, it can be seen that the magnetic permeability was significantly reduced and the fluidity was slightly reduced; combined with the test results of Example 8, when the vinyl ferrocene-acrylate polymer was replaced with an acrylic resin, although the fluidity changed slightly, the magnetic permeability was significantly reduced. Combined with the test results of Example 7, when only polyamide resin was included in the outer coating layer in Example 7, the magnetic permeability was also significantly reduced, and the fluidity was also slightly reduced.

[0131] Referring to the test results of Example 1 and Example 9, when paraffin wax is used as the binder in Example 9, the magnetic permeability is significantly reduced compared with Example 1, and the fluidity is also slightly reduced; in combination with the test results of Examples 10-12, when aromatic aldehyde is added to the composite magnetic fluid, it can be seen that the magnetic permeability is further significantly improved. Combining the test results of Example 1 with Comparative Examples 1 and 2, the amount of binder added in Comparative Example 2 is increased, and the magnetic permeability decreases significantly, while in Comparative Example 1, when the amount of binder added is reduced and the amount of ferrite powder is increased, the magnetic permeability is improved, but the fluidity is greatly reduced.

[0132] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A method for preparing an inductor by composite magnetic fluid integral injection molding, characterized in that: The following steps are involved: S1. Preparation of high magnetic permeability composite magnetic fluid: mixing ferrite powder with a binder and a dispersant to obtain a composite magnetic fluid, and then grinding and removing impurities; S2, cleaning and drying the inductor coil (1) obtained by winding the high-conductivity metal wire; S3, placing the inductor coil (1) in step S2 in an injection mold, and then injecting the composite magnetic fluid after the impurities are removed in step S1 into the mold by injection molding to form a shell (2), thereby obtaining an inductor; The binder comprises paraffin wax and magnetic polymer microcapsules in a mass ratio of 1:(0.4-0.6), wherein the magnetic polymer microcapsules comprise a core material, an inner coating layer and an outer coating layer arranged in sequence from the inside to the outside, the core material comprises a ferric cyanide complex and a nickel-iron composite powder, the inner coating layer comprises a vinyl ferrocene-acrylate polymer, and the outer coating layer comprises a COPNA resin and a polyamide resin; In the composite magnetic fluid raw material, the addition amount of each raw material is as follows in parts by weight: 91-95 parts of ferrite powder, 4-6 parts of binder, and 1-3 parts of dispersant; The dispersant is selected from one or more of fatty alcohol polyoxyethylene ether, lignin sulfonate, and p-methoxy fatty amide benzene sulfonic acid.

2. The method for preparing an inductor by composite magnetic fluid integral injection molding according to claim 1, characterized in that: The vinyl ferrocene-acrylate polymer is prepared by the following method: 1) Add vinyl ferrocene, methyl methacrylate, acrylamide, maleic anhydride and initiator into tetrahydrofuran, stir and mix to prepare a monomer mixture; 2) Add stabilizer and ethylene glycol dimethacrylate to the monomer mixture, and then react at 80-90°C for 2-3h, then stop heating, cool to room temperature, centrifuge, and wash with water to obtain vinyl ferrocene-acrylate polymer.

3. The method for preparing an inductor by composite magnetic fluid integral injection molding according to claim 2, characterized in that: When preparing the vinyl ferrocene-acrylate polymer, each raw material is added according to the following weight parts: 10-20 parts of tetrahydrofuran, 15-25 parts of vinylferrocene, 15-25 parts of methyl methacrylate, 10-15 parts of acrylamide, 15-20 parts of maleic anhydride, 1-3 parts of initiator, 1-3 parts of stabilizer and 3-5 parts of ethylene glycol dimethacrylate.

4. The method for preparing an inductor by composite magnetic fluid integral injection molding according to claim 1, characterized in that: The ferric cyanide complex is prepared by the following method: Dissolving ferric chloride in water to prepare a ferric chloride solution with a mass concentration of 35-45%; Dissolving sodium cyanide in water to prepare a sodium cyanide solution with a mass concentration of 25-35%; Then, the sodium cyanide solution is poured into the ferric chloride solution and reacted for 40-60 minutes, then filtered and washed with water to obtain the ferric cyanide complex.

5. The method for preparing an inductor by composite magnetic fluid integral injection molding according to claim 1, characterized in that: The magnetic polymer microcapsules are prepared by the following method: The ferric cyanide complex and the nickel-iron composite powder are mixed and granulated to obtain core material particles, and then the vinyl ferrocene-acrylate polymer is dissolved in ethanol and sprayed on the surface of the core material as an inner coating solution, and dried to form an inner coating layer, and then COPNA resin and polyamide resin are dissolved in ethanol and sprayed on the inner coating layer as an outer coating solution, and dried to obtain magnetic polymer microcapsules; The mass ratio of the ferric cyanide complex to the nickel-iron composite powder is 1:(1.5-1.8), and the mass ratio of the COPNA resin to the polyamide resin is 1:(2-3); The added mass ratio of the core material particles to the inner coating layer solution is 1:(1.5-2), and the added mass ratio of the core material particles to the outer coating layer solution is 1:(1.2-1.5).

6. The method for preparing an inductor by composite magnetic fluid integral injection molding according to claim 1, characterized in that: 1-3 parts by weight of aromatic aldehyde are also added to the composite magnetic fluid.

7. An inductor obtained by the preparation method according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Plastic for injection molding of mutual inductor shells

    CN104292614A

  • Magneto-calorific curing method for thermosetting resin adhesive

    CN104312510A

  • Aerogel core material capsule, paint prepared from same and preparation method of paint

    CN105363396A

  • Soft magnetic composite material for integrated injection molded inductor and preparation method thereof

    CN107778847A

  • Composition for injection molding and sintered material obtained therefrom

    JP1991150257A