A thermoelectric cotton thread with an inorganic silver selenide-silver alternating structure and a preparation method thereof
By forming an inorganic silver selenide-silver alternating structure in the thermoelectric cotton thread, the problems of complex manufacturing process and low thermoelectric performance of flexible thermoelectric fibers are solved, enabling wearable devices with efficient energy harvesting and temperature sensing.
Patent Information
- Application Number
- CN202410564064.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-05-08
AI Technical Summary
In the existing technology, the preparation process of flexible thermoelectric fibers is complicated and the thermoelectric performance is low. Traditional semiconductor thermoelectric materials are difficult to attach to textile materials, which limits their application in wearable electronic devices.
Using the Torrens reaction and selenization method, silver nanoparticles and silver selenide nanoparticles are attached to cotton thread in segments to form an inorganic silver selenide-silver alternating structure thermoelectric cotton thread. This thread is then woven into textiles through weaving, sewing and other processes to form a flexible wearable thermoelectric device.
The prepared thermoelectric cotton wire has high output power, is lightweight and soft, and is suitable for wearable devices such as flexible temperature sensors and touch sensors, realizing efficient energy harvesting and temperature sensing.
Smart Images

Figure CN118510365B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermoelectric conversion, and in particular to a thermoelectric cotton thread with an inorganic silver selenide-silver alternating structure and a preparation method thereof. Background Art
[0002] In recent years, electronic textiles have the capabilities of sensing, communication and energy harvesting by integrating different functional yarns and electronic components. However, it is a huge challenge to drive multifunctional electronic textiles sustainably and stably. Recently, wearable energy harvesting systems based on thermoelectricity, piezoelectricity and triboelectricity have been widely used in wearable electronic devices. For thermoelectric materials, the Seebeck effect enables thermoelectric materials to directly convert the temperature difference between the human body surface temperature and the surrounding environment into voltage, providing continuous energy for wearable electronic devices. At the same time, they can also be used as temperature sensors for touch sensing, health detection and high temperature warning.
[0003] At present, common flexible thermoelectric fibers are usually prepared by wet spinning, soaking and other methods of organic thermoelectric materials, which have the disadvantages of complex process and low thermoelectric performance. At the same time, traditional semiconductor thermoelectric materials such as Bi2Te3 are difficult to attach to common textile materials such as cotton and polyester. Therefore, it is necessary to develop a simple process to attach traditional semiconductor thermoelectric materials to textile fibers to prepare flexible thermoelectric fibers, so as to promote the application of semiconductor thermoelectric materials in flexible thermoelectric fibers. Summary of the invention
[0004] In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a thermoelectric cotton thread with an inorganic silver selenide-silver alternating structure and a preparation method thereof. The thermoelectric cotton thread is prepared by attaching silver nanoparticles and silver selenide nanoparticles to the cotton thread in sections through "Torrance reaction" and "selenization" to prepare a thermoelectric cotton thread with an inorganic silver selenide-silver alternating structure. The thermoelectric cotton thread has good flexibility and can be woven into textiles through weaving, sewing, knitting and other processes. The obtained electronic device has good flexibility, air permeability and wearability, and has broad application prospects.
[0005] In order to achieve the above-mentioned object, the present invention provides a thermoelectric cotton wire having an inorganic silver selenide-silver alternating structure, wherein the thermoelectric cotton wire comprises a P-type silver cotton wire segment, an N-type silver selenide cotton wire segment, a conductive layer and a polymer encapsulation layer (such as Figure 1As shown in the figure, through the "Torrance reaction", silver nanoparticles are in situ grown on the surface of cotton fibers in the cotton thread to form a P-type silver cotton thread; then through "selenization", silver selenide nanoparticles are attached to the cotton fiber surface of some cotton thread segments in the P-type silver cotton thread to form N-type silver selenide cotton thread segments; thus, on a cotton thread, the P-type silver cotton thread segments and the N-type silver selenide cotton thread segments are respectively used as a section of the cotton thread to form an alternating structure in the form of alternating appearance; and, a low-temperature conductive adhesive is used as a connecting material to form a conductive layer between the P-type silver cotton thread segments and the N-type silver selenide cotton thread segments; finally, a polymer is used as an encapsulation material to form an encapsulation layer.
[0006] Furthermore, the cotton thread is replaced by any one of nylon, silk, and wool, and / or the polymer is polydimethylsiloxane (PDMS), and / or the low-temperature conductive adhesive is any one of conductive copper paste, conductive silver ink, and conductive silver paste.
[0007] The present invention also provides a method for preparing a thermoelectric cotton thread having an inorganic silver selenide-silver alternating structure, comprising the following steps:
[0008] Step S0, cotton thread pretreatment: first, the cotton thread was soaked in a dopamine (2 mg / ml) solution for 12 h, then washed with deionized water for multiple times, and finally, the treated cotton thread was naturally dried for later use.
[0009] Step S1, in-situ growth of silver nanoparticles: silver nanoparticles are in-situ grown on the surface of the cotton thread obtained in step S0 through the "Torrance reaction", and the cotton thread is repeatedly washed with deionized water and dried to obtain silver cotton thread.
[0010] Step S2, preparation of N-type selenide silver cotton thread segments: spirally wind the silver cotton thread obtained in step S1 on the surface of a ruler-shaped acrylic plate, and cover the silver cotton thread on either side of the ruler-shaped acrylic plate with Ecoflex 0030 for protection (e.g. Figure 4 d). Then, the ruler-shaped acrylic plate spirally wrapped with silver cotton thread is immersed in a selenium solution (refer to prior art documents 1, 3, 4) for "selenization" (refer to prior art documents 2, 3), and silver selenide nanoparticles are grown in situ on the surface of the silver cotton thread not covered by Ecoflex 0030 to form a silver selenide cotton thread segment; that is, the surface of the obtained cotton thread forms an Ag-Ag2Se alternating structure of silver nanoparticles and silver selenide nanoparticles (such as Figure 4 d).
[0011] Step S3, peeling the cotton thread with the Ag-Ag2Se alternating structure obtained in step S2 from the surface of the ruler-shaped acrylic plate, and removing the cured Ecoflex 0030 adhered to the surface of the cotton thread; then, applying a low-temperature conductive adhesive on the junction of the silver cotton thread segment and the silver selenide cotton thread segment of the cotton thread, and forming a conductive layer after drying.
[0012] Step S4, encapsulating the cotton thread obtained in step S3 with a polymer, thereby obtaining the thermoelectric cotton thread having an inorganic silver selenide-silver alternating structure.
[0013] The obtained thermoelectric cotton thread with an inorganic silver selenide-silver alternating structure is woven into fabric using weaving, sewing, textile and other processes to form a flexible wearable thermoelectric device.
[0014] Furthermore, in step S0, in addition to cotton thread, it can also be one of nylon, silk, and wool; the preparation method of the dopamine solution is: in deionized water, dopamine hydrochloride and tris(hydroxymethyl)aminomethane are added in sequence, and magnetic stirring is performed until completely dissolved; the soaking time is not less than 12 hours.
[0015] Furthermore, in step S1, the preparation method of the silver ammonia solution participating in the "Torrance reaction" is: slowly add silver nitrate and polyvinyl pyrrolidone into deionized water in sequence, stir magnetically until completely dissolved, and then add ammonia water with a concentration of 5 mol / L until the solution becomes clear.
[0016] Furthermore, the specific process of step S1 is: soaking the pretreated cotton thread in the silver ammonia solution for 20 minutes, then adding glucose monohydrate, stirring thoroughly and then standing to react for 1 to 3 hours.
[0017] Furthermore, step S1 also includes repeatedly performing the "Torrance reaction" 1-4 times, so that silver nanoparticles are in situ grown on the surface of the cotton thread 1-4 times.
[0018] Further, in step S2, Figure 4 The ruler-shaped acrylic plate shown has a length×width×height of 7 cm×1 cm×0.1 cm.
[0019] Furthermore, in step S2, the selenium solution is prepared by adding selenium powder and sodium sulfide nonahydrate into deionized water and mixing them; preferably, the selenium solution is prepared by sequentially adding 0.6 g of sodium sulfide nonahydrate and 0.2 g of selenium powder into 30 ml of deionized water, and magnetically stirring for 10 min.
[0020] Furthermore, in step S2, the specific process of spirally winding the silver cotton thread on the surface of the ruler-shaped acrylic plate is as follows: one end of the silver cotton thread obtained in step 1 is fixed to one end of the ruler-shaped acrylic plate with a clip, and then the silver cotton thread is spirally wound on the surface of the ruler-shaped acrylic plate, and then the other end of the silver cotton thread is also fixed to the other end of the ruler-shaped acrylic plate with a clip (such as Figure 4 After the operation is completed, the silver cotton thread is spirally wound on the surface of both sides of the ruler-shaped acrylic plate, and the silver cotton thread on the surface of either side of the ruler-shaped acrylic plate is coated with Ecoflex, and then placed in an oven for curing at 60°C for 30 minutes; after curing, remove the clip (as shown in FIG. Figure 4c), silver cotton threads are spirally wound on the surfaces of both sides of a ruler-shaped acrylic plate, wherein the silver cotton thread on the side not covered by Ecoflex is exposed for subsequent selenization, while the silver cotton thread on the other side covered by Ecoflex (i.e. encapsulated by Ecoflex) is prevented from contacting with the selenium solution during the subsequent selenization process.
[0021] Furthermore, in step S2, the specific process of "selenization" is: immersing a ruler-shaped acrylic plate with silver cotton thread spirally wound on the surface into a selenium solution for 4 hours, taking it out and repeatedly washing it with deionized water, and then drying it, so that an Ag-Ag2Se alternating structure of silver nanoparticles and silver selenide nanoparticles is formed on the surface of the cotton thread (such as Figure 4 d).
[0022] Furthermore, in step S3, the low-temperature conductive adhesive is any one of conductive copper paste, conductive silver ink, and conductive silver paste.
[0023] Furthermore, in step S3, the specific process of peeling the cotton thread with an Ag-Ag2Se alternating structure obtained in step S2 from the surface of the ruler-shaped acrylic plate and removing the cured Ecoflex 0030 adhered to the surface of the cotton thread is: pulling one end of the thermoelectric cotton thread obtained by mechanical peeling to pass through the hole of the panel, and continuing to pull the thermoelectric cotton thread until the other end also passes through the hole, and the cured Ecoflex adhered to the surface of the thermoelectric cotton thread is scraped off.
[0024] Furthermore, in step S4, the specific process of the cotton thread obtained in the polymer encapsulation step S3 is: immersing the cotton thread with the Ag-Ag2Se alternating structure into the PDMS solution, then taking it out, hanging the cotton thread vertically above, and forming a uniform PDMS film on the surface of the cotton thread under the action of gravity.
[0025] The present invention also provides an application of the thermoelectric cotton thread having an inorganic silver selenide-silver alternating structure, which is used as a raw material for preparing wearable electronic devices, flexible electronic devices, and electronic skin.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] 1. The present invention uses textile fibers such as cotton thread as a carrier, and grows inorganic thermoelectric materials in situ on the cotton thread through the Torrens reaction and selenization method to form an alternating structure. The obtained thermoelectric cotton thread has the characteristics of high output power, light weight, soft texture, good reliability, etc.
[0028] 2. The thermoelectric cotton thread of the present invention can be processed onto fabric through weaving, sewing and other processes to power wearable devices such as flexible temperature sensors, flexible touch sensors, etc.
[0029] Prior art document 1: Kolb, ED et al. The solubility of trigonal Se in Na2S solution and the hydrothermal growth of Se. J. Cryst. Growth. 8, 191 (1971).
[0030] Prior art document 2: Gates, B. et al. Synthesis and characterization ofcrystalline Ag2Se nanowires through a template-engaged reaction at roomtemperature. Adv. Funct. Mater. 12, 679 (2002).
[0031] Prior art document 3: Liu, YJ et al. Scalable-produced 3D elasticthermoelectric network for body heat harvesting. Nature Communications. 14, 3058 (2023).
[0032] Prior art document 4: CN105566190A. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a physical picture of the thermoelectric cotton thread with an inorganic silver selenide-silver alternating structure obtained at the end of the embodiment.
[0034] Figure 2 This is a physical picture of the thermoelectric device prepared by weaving technology.
[0035] Figure 3 In the figure, A is a physical picture of a thermoelectric device prepared by sewing technology, and B is a schematic diagram of the structure of thermoelectric cotton threads sewn on fabric to form electrical series and thermal parallel connection.
[0036] Figure 4 middle, Figure 4 a is a schematic diagram of a ruler-shaped acrylic plate; Figure 4 b is a physical picture of the ruler-shaped acrylic plate; Figure 4 c is a schematic diagram of the step 3.1 of the embodiment in which the silver cotton thread is spirally wound on a ruler-shaped acrylic plate and encapsulated with Ecoflex0030: the left picture shows the side not coated with Ecoflex0030, and the right picture shows the side coated with Ecoflex0030; Figure 4d is a schematic diagram of the product after selenization: in the left figure, the color of the silver cotton thread segment on the side not covered by Ecoflex0030 turns black, while in the right figure, the color of the silver cotton thread segment on the side covered by Ecoflex0030 remains unchanged. Figure 4 e is the cured Ecoflex adhered to the surface of the scraped cotton thread.
[0037] Figure 5 It is a SEM image of the silver cotton thread obtained in step 2 of the embodiment, wherein the inset is a partial enlarged image of the SEM image of the silver cotton thread.
[0038] Figure 6 3 is a SEM image of the cotton thread segment with silver selenide nanoparticles attached in the thermoelectric cotton thread obtained in step 3 of the embodiment, wherein the inset is a partial enlarged image of the SEM image.
[0039] Figure 7 The electrical performance test is carried out on the thermoelectric textile formed by weaving the thermoelectric cotton thread obtained in the embodiment into the textile. The upper figure is a schematic diagram of the test method, and the lower figure is the electrical performance test result.
[0040] Figure 8 middle, Figure 8 a is a real photo of a 5×5 pixel touch panel prepared based on the thermoelectric cotton thread obtained in the example, wherein the thermoelectric cotton thread obtained in the example is woven into a textile; Figure 8 b is the signal output by the touch panel when the finger touches the (3,3) node of the touch panel; Figure 8 c is the circuit diagram of a 5×5 pixel touch panel: the pixels are independent of each other, and each pixel is controlled individually by the control circuit; Figure 8 d is a real photo of “WHU” being written on the touch pad; Figure 8 e is a schematic diagram of two L-shaped objects of different temperatures placed on the touch pad; Figure 8 f is Figure 8 The case shown in e is the final voltage mapping of the touch panel to the temperature and shape information of two L-shaped objects at different temperatures.
[0041] Fig. 9 In the figure, A is silver silk obtained by Torrance reaction of silk, and B is silver selenide silk obtained by sequentially undergoing Torrance reaction and selenization reaction. DETAILED DESCRIPTION
[0042] The present invention is further described below in conjunction with the accompanying drawings and embodiments. The present invention is not limited by the following embodiments, and the specific implementation method can be determined based on the technical solution of the present invention and actual conditions.
[0043] The following are the raw materials used in the examples:
[0044] The cotton thread was purchased from Binzhou Yuanke Textile Co., Ltd., and the average diameter of the cotton thread was 800 μm.
[0045] Silver nitrate (AgNO3, analytical grade) was purchased from Chengdu Kelun Chemical Co., Ltd. Ammonia solution (analytical grade) and glucose monohydrate (C6H 12 O6·H2O, analytical grade). Tris(hydroxymethyl)aminomethane (C4H 11 NO3, 99.8%), dopamine hydrochloride (98%), polyvinylpyrrolidone (PVP, average molecular weight ≈ 55000), sodium sulfide nonahydrate (Na2S·9H2O, 98%), selenium powder (Se, 99.9%). Polydimethylsiloxane (PDMS, Sylgard 184) purchased from Dow Corning, USA. Ecoflex (0030) purchased from Smooth-On, USA.
[0046] All purchased chemicals were used directly without further purification.
[0047] Preparation of dopamine solution: Add dopamine hydrochloride (0.08 g) and tris(hydroxymethyl)aminomethane (0.048 g) in 40 ml of deionized water, and stir magnetically until completely dissolved.
[0048] Preparation method of silver ammonia solution: add silver nitrate (0.9 g) and polyvinyl pyrrolidone (0.0045 g) to 30 ml of deionized water, and stir magnetically until completely dissolved; then measure ammonia water (5 mol / L) and slowly add it to the silver nitrate solution until the solution becomes clear.
[0049] Preparation method of selenium solution: In 30 ml of deionized water, add sodium sulfide nonahydrate (0.6 g) and selenium powder (0.2 g) in sequence and stir magnetically for 10 minutes.
[0050] The length×width×height of the acrylic plate used is 7cm×1cm×0.1cm.
[0051] Example
[0052] A method for preparing a thermoelectric cotton thread having an inorganic silver selenide-silver alternating structure comprises the following steps:
[0053] Step 1: Substrate pretreatment: First, soak the cotton thread in a dopamine solution for 12 hours, then wash it with deionized water for multiple times, and finally, dry the washed cotton thread naturally for later use.
[0054] Step 2, in-situ growth of silver nanoparticles: soak the cotton thread obtained in step 1 in a silver ammonia solution, so that the cotton thread is fully in contact with the silver ammonia solution, and soak for 20 minutes; then add glucose monohydrate (mass 1.8g) to the silver ammonia solution, stir it thoroughly, and let it stand for 1 hour; finally, wash the obtained cotton thread repeatedly with deionized water and dry it;
[0055] The dried cotton thread is then subjected to the above-mentioned operation of this step again to obtain the silver cotton thread.
[0056] Step 3: In-situ growth of silver selenide nanoparticles:
[0057] 3.1. Pre-processing of silver cotton thread: Fix one end of the silver cotton thread obtained in step 2 to one end of the ruler-shaped acrylic plate with a clip, then spirally wrap the silver cotton thread around the surface of the ruler-shaped acrylic plate, and then fix the other end of the silver cotton thread to the other end of the ruler-shaped acrylic plate with a clip (such as Figure 4 After the operation is completed, the silver cotton thread is spirally wound on the surface of both sides of the ruler-shaped acrylic plate, and the silver cotton thread on the surface of either side of the ruler-shaped acrylic plate is coated with Ecoflex, and then placed in an oven for curing at 60°C for 30 minutes; after curing, remove the clip (as shown in FIG. Figure 4 c), silver cotton threads spirally wound on the surfaces of both sides of the ruler-shaped acrylic plate, wherein the silver cotton thread on the side not covered by Ecoflex is exposed and used for subsequent selenization, while the silver cotton thread on the other side covered by Ecoflex (i.e., encapsulated by Ecoflex) is prevented from contacting with the selenium solution during the subsequent selenization process;
[0058] 3.2. Selenization: The silver cotton thread pre-processed in step 3.1 and the ruler-shaped acrylic plate are immersed in the selenium solution for 4 hours. After being taken out, they are repeatedly washed with deionized water and dried. The Ag-Ag2Se alternating structure of silver nanoparticles and silver selenide nanoparticles is formed on the surface of the cotton thread (such as Figure 4 d, as shown in 4e);
[0059] 3.3. Mechanically peeling the cotton thread with the Ag-Ag2Se alternating structure obtained in step 3.2 from the surface of the ruler-shaped acrylic plate, and then scraping off the solidified Ecoflex adhered to the surface of the cotton thread with the Ag-Ag2Se alternating structure;
[0060] In this embodiment, the tool used to scrape off the solidified Ecoflex adhered to the surface of the cotton thread is as follows: Figure 4 As shown in FIG. 5 , the operation process is as follows: one end of the cotton thread obtained by mechanical stripping is pulled to pass through the hole of the panel, and the cotton thread is continued to be pulled until the other end also passes through the hole, and the solidified Ecoflex adhered to the surface of the cotton thread is scraped off.
[0061] Step 4, encapsulation: coating the junction of the cotton thread segment with Ag nanoparticles attached and the cotton thread segment with Ag2Se nanoparticles attached in the cotton thread obtained in step 3 with conductive silver paste to form a silver conductive layer, which serves as a connecting electrode between the cotton thread segment with Ag nanoparticles attached and the cotton thread segment with Ag2Se nanoparticles attached; after the conductive silver paste is dried to form the silver conductive layer, evenly coating the surface of the cotton thread with PDMS solution for encapsulation, thereby obtaining the thermoelectric cotton thread with the inorganic silver selenide-silver alternating structure.
[0062] The thermoelectric cotton thread obtained in this embodiment is as follows Figure 1 As shown, the microscopic morphology of the cotton thread segment attached with silver nanoparticles and the cotton thread segment attached with silver selenide nanoparticles are shown as follows: Figure 5 , 6 As shown by Figure 5 , 6 As can be seen from the partial enlarged image in the middle, silver nanoparticles and silver selenide nanoparticles are evenly coated on the fiber surface of the cotton thread.
[0063] Sewing / Weaving Crafts:
[0064] The thermoelectric cotton thread obtained in the above embodiment is woven into the fabric through sewing / weaving process, and the obtained product is as follows Figure 2 , 3 shown.
[0065] like Figure 3 As shown, in order to demonstrate the energy collection effect of the thermoelectric cotton thread obtained in the above embodiment, it is woven into a textile with a thickness of 10 mm: a thermoelectric cotton thread is woven into the textile by a shuttle to obtain a thermoelectric textile including 50 pairs of P-type silver nanoparticles-N-type silver selenide nanoparticles, and the P-type silver nanoparticles, the N-type silver selenide nanoparticles and the silver conductive layer therebetween form a thermal parallel and electrical series structure; the electrical performance of the thermoelectric textile is tested (the test method is as follows Figure 7 The results are shown in the upper middle figure. Figure 7 The figure below shows the output voltage and power density of thermoelectric textiles at different temperature differences (ΔT): The power density and output voltage of thermoelectric textiles are proportional to ΔT. The thermoelectric textiles provide a maximum of 500 μW·m at ΔT = 30K. -2 power density and an output voltage of 110.53mV.
[0066] Figure 7The test method shown in the upper middle figure is: the thermoelectric textile obtained above is placed on a heating plate (corresponding to the hot end), and the other side is pressed with an aluminum block (corresponding to the cold end, transferring heat to keep the cold end at a low temperature for a long time) to enhance heat dissipation; thermocouples (Jinke multi-channel temperature tester JK-8C) are placed on the upper and lower ends of the thermoelectric textile respectively, and the temperature difference between the upper and lower sides (i.e., the cold end and the hot end) of the thermoelectric textile is measured; the two ends of the thermoelectric cotton thread (as electrode pins) are connected to the instrument (keithley2400), and the voltage of the thermoelectric textile under different temperature differences is measured, and the output power is calculated by the formula P=U*U / R (R is the resistance of the thermoelectric textile first measured during the test, which is 2.7KΩ).
[0067] Touch Sensor:
[0068] 25 identical segments of thermoelectric cotton thread were cut from the thermoelectric cotton thread obtained in the above embodiment, each segment of thermoelectric cotton thread included a segment of silver cotton thread, a segment of silver selenide cotton thread and a silver conductive layer therebetween, and then the 25 segments of thermoelectric cotton thread were sewn into the fabric (each segment of thermoelectric cotton thread was independent of each other and was controlled separately, and the signal generated by each segment of thermoelectric cotton thread was read independently, such as Figure 8 c), a 5×5 flexible thermoelectric array touch panel was prepared, which can sense the touch and movement trajectory of objects of different temperatures such as fingers.
[0069] like Figure 8 As shown in a, the geometric coordinates of each section of thermoelectric cotton thread are determined by defining the x-axis and y-axis of the longitude and latitude. Figure 8 b shows the signal generated by the thermoelectric cotton thread when the finger touches the node (3,3); it is worth noting that when the finger touches the thermoelectric cotton thread at (x-3, y-3), the thermoelectric cotton thread at that location generates a strong signal, while the signal response of the non-contact thermoelectric cotton thread is almost negligible. This result verifies the addressability of the contact position of the panel. The 5×5 pixel touch panel enables us to successfully input the handwritten letters "WHU", such as Figure 8 As shown in d. Figure 8 e is two L-shaped iron blocks of different temperatures placed on the touch panel, and the temperature and shape information of the two L-shaped iron blocks are reflected on the touch panel. Figure 8 f. Therefore, the touch panel prepared by the thermoelectric cotton thread with inorganic silver selenide-silver alternating structure based on the present invention has obvious potential in various application fields such as writing, communication, space positioning and shape sensing.
[0070] The above are only preferred embodiments of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, and these all fall within the protection scope of the present invention.
Claims
1. A thermoelectric cotton wire with an inorganic silver selenide-silver alternating structure, the thermoelectric cotton wire comprising a P-type silver cotton wire segment, an N-type silver selenide cotton wire segment, a conductive layer and a polymer encapsulation layer, characterized in that: Through the "Torrens reaction", silver nanoparticles are in situ grown on the surface of cotton fibers in the cotton thread to form a P-type silver cotton thread; and then through "selenization", silver selenide nanoparticles are attached to the cotton fiber surface of some cotton segments in the P-type silver cotton thread to form N-type silver selenide cotton segments; thus, on a cotton thread, the P-type silver cotton segments and the N-type silver selenide cotton segments are respectively used as a section of the cotton thread to form an alternating structure in the form of alternating appearance; and, a low-temperature conductive adhesive is used as a connecting material to form a conductive layer between the P-type silver cotton segments and the N-type silver selenide cotton segments; a polymer is used as a packaging material to form a packaging layer; the low-temperature conductive adhesive is any one of a conductive copper paste, a conductive silver ink, and a conductive silver paste.
2. The thermoelectric cotton thread according to claim 1, characterized in that The cotton thread is replaced by any one of nylon, silk, and wool, and / or the polymer is polydimethylsiloxane, and / or the low-temperature conductive adhesive is any one of conductive copper paste, conductive silver ink, and conductive silver paste.
3. A method for preparing a thermoelectric cotton thread with an inorganic silver selenide-silver alternating structure, comprising the following steps: Step S0, pretreatment of the cotton thread: first, soaking the cotton thread in a dopamine solution, then washing it with deionized water for multiple times, and finally, naturally drying the treated cotton thread for later use; Step S1, in-situ growth of silver nanoparticles: silver nanoparticles are in-situ grown on the surface of the cotton thread obtained in step S0 through the "Torrance reaction", and the cotton thread is repeatedly washed with deionized water and dried to obtain a silver cotton thread; Step S2, preparation of N-type selenide silver cotton thread segments: spirally wind the silver cotton thread obtained in step S1 on the surface of a ruler-shaped acrylic plate, and cover and protect the silver cotton thread on either side of the ruler-shaped acrylic plate with Ecoflex 0030; then, immerse the entire ruler-shaped acrylic plate spirally wound with the silver cotton thread in a selenium solution for "selenization", and in situ grow silver selenide nanoparticles on the surface of the silver cotton thread not covered by Ecoflex 0030 to form selenide silver cotton thread segments; that is, the surface of the obtained cotton thread forms an Ag-Ag2Se alternating structure of silver nanoparticles and silver selenide nanoparticles; Step S3, peeling the cotton thread with the Ag-Ag2Se alternating structure obtained in step S2 from the surface of the ruler-shaped acrylic plate, and removing the cured Ecoflex 0030 adhered to the surface of the cotton thread; then, applying a low-temperature conductive adhesive on the junction of the silver cotton thread segment and the silver selenide cotton thread segment of the cotton thread, and forming a conductive layer after drying; Step S4, encapsulating the cotton thread obtained in step S3 with a polymer, thereby obtaining the thermoelectric cotton thread having an inorganic silver selenide-silver alternating structure.
4. The preparation method according to claim 3, characterized in that: In step S0, the cotton thread is replaced by any one of nylon, silk and wool; and / or, the preparation method of the dopamine solution is: in deionized water, dopamine hydrochloride and tris(hydroxymethyl)aminomethane are added in sequence, and magnetic stirring is performed until the solution is completely dissolved; the soaking time is not less than 12 hours.
5. The preparation method according to claim 3, characterized in that: In step S1, the preparation method of the silver ammonia solution participating in the "Torrance reaction" is: silver nitrate and polyvinyl pyrrolidone are slowly added to deionized water in sequence, magnetically stirred until completely dissolved, and then ammonia water with a concentration of 5 mol / L is added until the solution becomes clear.
6. The preparation method according to claim 3, characterized in that: The specific process of step S1 is: soaking the pretreated cotton thread in the silver ammonia solution for 20 minutes, then adding glucose monohydrate, stirring thoroughly and then standing to react for 1 to 3 hours.
7. The preparation method according to claim 6, characterized in that: Step S1 also includes repeatedly performing the "Torrance reaction" 1-4 times, so that silver nanoparticles are in situ grown on the surface of the cotton thread 1-4 times.
8. The preparation method according to claim 3, characterized in that: In step S2, the selenium solution is prepared by adding selenium powder and sodium sulfide nonahydrate into deionized water and mixing them.
9. The preparation method according to claim 8, characterized in that: The preparation method of the selenium solution is as follows: 0.6 g of sodium sulfide nonahydrate and 0.2 g of selenium powder are added to 30 ml of deionized water in sequence, and magnetic stirring is performed for 10 minutes.
10. The preparation method according to claim 3, characterized in that: In step S2, the specific process of spirally winding the silver cotton thread on the surface of the ruler-shaped acrylic plate is as follows: fix one end of the silver cotton thread obtained in step S1 to one end of the ruler-shaped acrylic plate with a clip, then spirally wind the silver cotton thread on the surface of the ruler-shaped acrylic plate, and then fix the other end of the silver cotton thread to the other end of the ruler-shaped acrylic plate with a clip; after the operation is completed, the silver cotton thread is spirally wound on the surface of both sides of the ruler-shaped acrylic plate, and the silver cotton thread on the surface of either side of the ruler-shaped acrylic plate is coated with Ecoflex 0030, and then placed in an oven for curing at 60°C for 30 minutes; after curing, remove the clip, and spirally wind the silver cotton thread on the surface of both sides of the ruler-shaped acrylic plate, wherein the silver cotton thread on the side not covered by Ecoflex 0030 is exposed and used for subsequent selenization, and the silver cotton thread on the other side covered by Ecoflex 0030 is prevented from contacting with the selenium solution during the subsequent selenization process.
11. The preparation method according to claim 3, characterized in that: In step S2, the specific process of "selenization" is: immerse the ruler-shaped acrylic plate with silver cotton thread spirally wrapped on the surface into a selenium solution for 4 hours, take it out and repeatedly wash it with deionized water, and then dry it, so that an Ag-Ag2Se alternating structure of silver nanoparticles and silver selenide nanoparticles is formed on the surface of the cotton thread.
12. The preparation method according to claim 3, characterized in that: In step S3, the low-temperature conductive adhesive is any one of conductive copper paste, conductive silver ink, and conductive silver paste; the specific process of peeling the cotton thread with an Ag-Ag2Se alternating structure obtained in step S2 from the surface of the ruler-shaped acrylic plate and removing the cured Ecoflex 0030 adhered to the surface of the cotton thread is: pulling one end of the thermoelectric cotton thread obtained by mechanical peeling to pass through the hole of the panel, and continuing to pull the thermoelectric cotton thread until the other end also passes through the hole, and the cured Ecoflex 0030 adhered to the surface of the thermoelectric cotton thread is scraped off.
13. The preparation method according to claim 3, characterized in that: In step S4, the specific process of the cotton thread obtained in the polymer encapsulation step S3 is: immersing the cotton thread with the Ag-Ag2Se alternating structure into the polydimethylsiloxane solution, then taking it out, hanging the cotton thread vertically above, and forming a uniform polydimethylsiloxane film on the surface of the cotton thread under the action of gravity.
14. Use of the thermoelectric cotton thread with an inorganic silver selenide-silver alternating structure according to any one of claims 1-2 or the thermoelectric cotton thread with an inorganic silver selenide-silver alternating structure prepared by the preparation method according to any one of claims 3-13 in the preparation of flexible electronic devices.
15. The use according to claim 14, characterized in that: The flexible electronic device is a wearable electronic device or an electronic skin; the process for preparing the flexible electronic device is weaving, sewing, or textile, and the thermoelectric cotton thread is woven into the cloth to form the flexible electronic device.