A visual anti-adhesion, drag-reducing and injury-free tunnel needle and its preparation method and application
The visual anti-adhesion, drag-reducing and injury-free tunnel needle prepared by stainless steel materials and high-precision processing technology solves the problems of adhesion and resistance of traditional tunnel needles in the process of establishing tunnels, improves operating efficiency and safety, and has a better development effect. Better, reducing the risk of complications.
Patent Information
- Application Number
- CN202411007545.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Traditional tunnel needles have safety issues such as adhesion, high running resistance, accidental injury to blood vessels or nerves, and easy detachment of catheters during the process of establishing tunnels. The operation is also complicated, which limits their wide application in medical practice.
The visual anti-adhesion, drag-reducing and injury-free tunnel needle is made of stainless steel. The material toughness is improved through heating, water quenching, tempering, fine grinding and other processes. It is combined with three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser processing to form micro-nano structures and prepare the tip. The dual-stage gradient structure and blunt-end structure increase friction and self-cleaning properties, and the anodizing process improves the mirror effect and develops clearer images.
It realizes the self-cleaning and anti-adhesion of the tunnel needle, reduces the resistance during use, improves the operating efficiency and safety, makes the imaging more significant, improves the accuracy and safety of the operation, and reduces the incidence of complications.
Smart Images

Figure CN118512243B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of medical devices, and in particular to a visualized anti-adhesion, drag-reducing and injury-free tunnel needle, and a preparation method and application thereof. Background Art
[0002] A peripherally inserted central catheter (PICC) is a catheter inserted through a peripheral vein, with the tip of the catheter positioned in the superior vena cava or inferior vena cava. It has the advantages of less trauma, easy operation, long retention time, and avoidance of drug extravasation. It is widely used in intravenous nutrition, tumor chemotherapy, antibiotic treatment and other fields, providing a safe and reliable channel for intravenous infusion for patients. However, the incidence of total complications of traditional non-tunnel PICC catheterization is relatively high. Tunneling technology is a technology for subcutaneous catheterization, which avoids the direct connection of the catheter in traditional catheterization to the blood vessel, thereby reducing bleeding and exudation, and reducing the incidence of catheter-related complications.
[0003] Tunnel needle is an important tool for subcutaneous medical operations, such as establishing a subcutaneous tunnel to introduce catheters or other medical devices in interventional surgery. Traditional tunnel needles often face safety issues such as adhesion, high running resistance, accidental injury to blood vessels or nerves, and easy detachment of the catheter during tunnel establishment. In addition, the entire operation process places strict requirements on medical workers, which limits its widespread application in medical practice.
[0004] At present, in order to solve the above problems of tunnel needles, various improvement methods have been proposed. For example, Chinese patent CN110960298 B discloses a subcutaneous tunnel establishment tool for tunnel-type PICC catheterization, which includes a tunnel needle and a needle body push rod. The PICC catheter passes through the inside of the tunnel needle needle tube, which can avoid the possibility of the edge of the end of the PICC catheter scratching the subcutaneous tissue or blood vessels, so that the PICC catheter can pass through the subcutaneous tunnel quickly. However, its structure is complex, the method of use is cumbersome, the probability of failure during use is high, and the tunnel establishment process is not visible, and there are still safety hazards. Chinese patent CN214128714 U discloses a subcutaneous tunnel establishment component for tunnel-type PICC catheterization, which can avoid the fall of the catheter and reduce stimulation, but the tunnel establishment is still invisible and has high resistance. The requirements for medical workers are still high, and the needle tip is large, which is likely to tear the catheter. The cracked catheter edge may then scratch other tissues such as blood vessels, resulting in surgical errors.
[0005] Therefore, a new design and preparation method that can comprehensively solve the problems of existing tunnel needles is needed to improve the practicality and wide applicability of tunnel needles in subcutaneous operations. The emergence of the present invention is an innovative solution proposed to solve these technical challenges, aiming to improve the operating efficiency, safety and visual controllability of tunnel needles, thereby promoting the progress of medical practice. Summary of the invention
[0006] One of the purposes of the present invention is to provide a visual anti-adhesion, drag-reducing and injury-free tunnel needle in order to solve the above-mentioned technical problems.
[0007] The second object of the present invention is to provide a method for preparing a visualized anti-adhesion, drag-reducing and injury-free tunnel needle, which is carried out according to the following operating steps:
[0008] (1) Preparation of tunnel needle substrate: Select stainless steel material, perform rough grinding, heating, water quenching, tempering, cooling, and fine grinding;
[0009] To better implement the present invention, further, the stainless steel material is one of 06Cr19Ni10, 06Cr17Ni12Mo2, 00Cr19Ni10, and 00Cr17Ni14Mo2;
[0010] To better implement the present invention, further, the heating temperature is 700-1000°C and the duration is 1-5 min;
[0011] To better implement the present invention, further, the tempering temperature is 450-650°C and the duration is 30-60 min;
[0012] (2) Preparation of surface micro-nanostructure: select the tunnel needle substrate, rinse with flowing purified water, ultrasonically clean with mixed organic solution, and ultrasonically clean with purified water; treat the surface with cold atmospheric pressure plasma and blow dry with clean air; preheat, perform three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser on the middle needle body, and immediately transfer it to a nitrogen and oxygen environment for high-temperature treatment, followed by secondary water quenching, and then ultrasonic cleaning with purified water;
[0013] To better implement the present invention, further, the mixed organic solution is an anhydrous ethanol and acetone solution with a volume ratio of 1:1, and the ultrasonic cleaning time is 15 min;
[0014] To better implement the present invention, further, the gas used for the cold atmospheric pressure plasma treatment is one or both of argon and helium;
[0015] To better implement the present invention, further, the preheating temperature is 40-90°C;
[0016] To better realize the present invention, further, the three-dimensional ultrasonic nitrogen jet is to combine the ultrasonic system, the nitrogen emission system and the three-dimensional motion system to reduce the fallback and adhesion of the laser ablation products generated by the femtosecond laser in the laser working area on the surface of the tunnel needle;
[0017] To better implement the present invention, further, the femtosecond laser parameters are a pulse width of 25-350 fs, a wavelength of 250-800 nm, and a laser energy density of 0.05-1.5 J / cm 2 , pulse frequency of 1-250 kHz, diameter of the focused laser beam of 25 µm;
[0018] To better implement the present invention, further, the nitrogen-oxygen environment is an environment formed by a mixture of nitrogen and oxygen in a volume ratio of 3-5:1, and the high temperature treatment temperature is 100-300° C. and the duration is 2-10 h;
[0019] (3) Preparation of the tip double-stage gradient structure and blunt-end structure: preheating the needle body, CNC lathe cutting, and then ultrasonic cleaning with mixed organic solution and purified water;
[0020] To better implement the present invention, further, the preheating temperature is 40-90° C., and the ultrasonic cleaning time is 15 min;
[0021] To better implement the present invention, further, the mixed organic solution is an anhydrous ethanol and acetone solution with a volume ratio of 1:1, and the ultrasonic cleaning time is 15 min;
[0022] (4) Special treatment of the structures at both ends: fix the middle needle body and perform anodizing on the structures at both ends; ultrasonic type performs CNC lathe cutting on the basis of anodizing to prepare annular grooves;
[0023] To better implement the present invention, further, the anodic oxidation, oxidation time is 1-3 min, the voltage is 45-65V;
[0024] (5) Preparation of visualized anti-adhesion, drag-reducing and damage-free tunnel needle: The needle tip is made into a smooth and blunt structure through fine grinding, and then ultrasonically cleaned with purified water to obtain a tunnel needle.
[0025] Beneficial effects of the present invention:
[0026] 1. Structure itself: The tunnel needle is composed of a straight solid stainless steel, does not contain other connectors, does not add any other coatings, and will not cause abnormal situations such as disconnection and coating allergies; the middle needle body is the main part of the tunnel needle, and its surface is a micro-nano-level rib structure, which can achieve self-cleaning and anti-adhesion while reducing use resistance and improving operation efficiency; the ultrasonic type has a roughened structure at both ends, and a reflector is added, which makes the image clearer and the visualization more significant, so that the operator can clearly observe the position and shape of the subcutaneous tunnel; the tip is a two-stage gradient structure, and each stage is transitioned by a spherical arc surface, which can increase the friction between the catheter, prevent the catheter from slipping, improve the stability of use, and improve the smoothness of tunnel establishment; the tip of the needle has a smooth and blunt structure, which automatically avoids blood vessels, nerves and other tissues to avoid accidental injuries and improve surgical safety;
[0027] 2. Preparation process: Heating, water quenching and tempering the stainless steel material can improve the toughness and ductility of the material, making it more suitable for subsequent processing and use; cold atmospheric pressure plasma treatment of the tunnel needle substrate surface can make it easier to interact with the laser and improve the bonding strength; preheating can reduce thermal stress and deformation, and avoid cracks or other damage to the material during laser treatment; since laser material removal cannot avoid the removal of the material falling back to the processed surface to form a recast layer, three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser can blow the laser ablation product away from the tunnel needle surface, reducing its fall and adhesion in the laser working area on the tunnel needle surface, so as to improve the laser processing efficiency and microstructure quality. In addition, under the action of the laser, nitrogen will dissolve into the surface of the stainless steel body, which can improve the strength and corrosion resistance; high temperature treatment in a nitrogen and oxygen environment after laser treatment can improve oxidation resistance, and secondary water quenching can further consolidate the mechanical properties of the tunnel needle;
[0028] 3. Application: At present, most clinical operations such as tissue perforation, access establishment, and subcutaneous tunnel establishment are performed blindly, which is too dependent on the experience and skills of medical workers. Visualization of the process can effectively improve the accuracy and safety of surgical operations; BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Front view of type I visual anti-adhesion, drag-reducing and injury-free tunnel needle
[0030] Figure 2 Front view of type II visual anti-adhesion, drag-reducing and injury-free tunnel needle
[0031] Figure 3 Front view of type III visual anti-adhesion, drag-reducing and injury-free tunnel needle
[0032] Figure 4 Front view of type IV visual anti-adhesion, drag-reducing and injury-free tunnel needle
[0033] Figure 5Longitudinal section of the roughened tip of the tunnel needle for visualization of anti-adhesion, drag reduction and damage prevention
[0034] Figure 6 Longitudinal section of the blunt end of the roughened tunnel needle for visualization of anti-adhesion, drag-reducing and injury-free tunnel needle
[0035] Figure 7 Schematic diagram of the top view of the micro-nano rib structure on the surface of the middle needle body of the tunnel needle for visualizing the anti-adhesion, drag reduction and injury prevention
[0036] Figure 8 Schematic diagram of the front view of the micro-nano rib structure on the surface of the middle needle body of the tunnel needle for visualizing the anti-adhesion, drag reduction and injury prevention
[0037] Fig. 9 Schematic diagram of the cross-section of the micro-nano rib structure on the surface of the middle part of the tunnel needle for visualizing the anti-adhesion, drag-reducing and injury-free tunnel needle
[0038] Fig.10 Diagram of the animal test process for establishing a subcutaneous tunnel for ultrasonic tunnel needle
[0039] Fig.11 This is the result of ultrasound detection of the tunnel needle in the animal's subcutaneous tunnel, where a is the standard type and b is the ultrasound type
[0040] Fig.12 Schematic diagram of two subcutaneous tunnel establishment methods, where c is an antegrade tunnel and d is a retrograde tunnel
[0041] Figure numerals: A, two-end structure, B, middle needle body, 1, standard tip structure, 2, standard blunt end structure, 3, ultrasonic tip structure, 4, ultrasonic blunt end structure, 5, surface micro-nano structure, 6, tip double-stage gradient structure, 7, annular groove, 8, needle smooth blunt structure, 9, secondary gradient structure, 10, spherical arc surface structure, 11, primary gradient structure, 12, brick-like structure, 13, convex point structure, DETAILED DESCRIPTION
[0042] The technical scheme of the present invention is further described in detail below in conjunction with embodiments and comparative examples, but the present invention is not limited to these specific embodiments.
[0043] The following are examples and comparative examples.
[0044] Example 1
[0045] Stainless steel material was selected, coarsely ground, heated to 850℃ and maintained for 3 min, quenched in water, placed in a 550℃ environment for 45 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; preheated to 65℃, and then the middle needle body B was subjected to three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser, with laser parameters of pulse width 164 fs, wavelength 780 nm, and laser energy density 1.32 J / cm 2 , pulse frequency 1kHz, focused laser beam diameter 25 µm, immediately transferred to nitrogen and oxygen (volume ratio 4:1) environment for 200℃ treatment for 6 h, then immediately water quenched for the second time, and then ultrasonically cleaned with purified water for 15 min to obtain a surface micro-nano structure 5 containing a brick-like structure 12 and a bump structure 13; the needle body was preheated to 65℃, and a standard tip structure 1 and a standard blunt end structure 2 were prepared by CNC lathe cutting, wherein the standard tip structure 1 is also called a tip double-stage gradient structure 6, which includes a secondary gradient structure 9, a spherical arc surface structure 10 and a primary gradient structure 11, and then ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the middle needle body B was fixed, and the structures A at both ends were anodized at a voltage of 50V 2 min, wherein the ultrasonic type is subjected to CNC lathe cutting processing on the basis of anodizing to prepare an annular groove 7, thereby obtaining an ultrasonic tip structure 3 and an ultrasonic blunt end structure 4; finally, a needle tip smooth blunt structure 8 is prepared by fine grinding, and then ultrasonic cleaning with purified water for 15 min is performed to obtain a visualized anti-adhesion, drag-reducing and damage-free tunnel needle.
[0046] Example 2
[0047] Stainless steel material was selected, coarsely ground, heated to 700℃ and maintained for 5 min, quenched in water, placed in a 450℃ environment for 60 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; preheated to 40℃, and then the middle needle body B was subjected to three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser, with laser parameters of pulse width 35 fs, wavelength 800 nm, and laser energy density 0.7 J / cm 2, pulse frequency 1kHz, focused laser beam diameter 25 µm, immediately after completion transferred to nitrogen and oxygen (volume ratio 3:1) environment for 100 ℃ treatment for 10 h, then immediately secondary water quenching, and then purified water ultrasonic cleaning for 15 min, to obtain a surface micro-nano structure 5 containing a brick-like structure 12 and a bump structure 13; the needle body was preheated to 40 ℃, and a standard tip structure 1 and a standard blunt end structure 2 were prepared by CNC lathe cutting, and then ultrasonic cleaning was carried out in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then purified water ultrasonic cleaning for 15 min; the middle needle body B was fixed, and the two end structures A were anodized at 45V for 3 min, in which the ultrasonic type was CNC lathe cutting on the basis of anodizing to prepare an annular groove 7, to obtain an ultrasonic tip structure 3 and an ultrasonic blunt end structure 4; finally, a smooth blunt structure 8 of the needle tip was prepared by fine grinding, and then purified water ultrasonic cleaning was carried out for 15 min to obtain a visualized anti-adhesion drag reduction and damage-free tunnel needle.
[0048] Example 3
[0049] Stainless steel material was selected, coarsely ground, heated to 1000℃ and maintained for 1 min, quenched in water, placed in a 650℃ environment for 30 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; preheated to 90℃, and then the middle needle body B was subjected to three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser, with laser parameters of pulse width 30 fs, wavelength 800 nm, and laser energy density 0.55 J / cm 2 , pulse frequency 1kHz, focused laser beam diameter 25 µm, immediately after completion transferred to nitrogen and oxygen (volume ratio 5:1) environment for 300℃ treatment for 2 h, then immediately secondary water quenching, and then purified water ultrasonic cleaning for 15 min, to obtain a surface micro-nano structure 5 containing a brick-like structure 12 and a bump structure 13; the needle body was preheated to 90℃, and a standard tip structure 1 and a standard blunt end structure 2 were prepared by CNC lathe cutting, and then ultrasonic cleaning was carried out in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then purified water ultrasonic cleaning for 15 min; the middle needle body B was fixed, and the two end structures A were anodized at 65V for 1 min, in which the ultrasonic type was CNC lathe cutting on the basis of anodizing to prepare an annular groove 7, to obtain an ultrasonic tip structure 3 and an ultrasonic blunt end structure 4; finally, a smooth blunt structure 8 of the needle tip was prepared by fine grinding, and then purified water ultrasonic cleaning was carried out for 15 min to obtain a visualized anti-adhesion drag reduction and damage-free tunnel needle.
[0050] Example 4
[0051] Stainless steel material was selected, coarsely ground, heated to 700℃ and maintained for 5 min, quenched in water, placed in a 550℃ environment for 45 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; preheated to 90℃, and then the middle needle body B was subjected to three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser, with laser parameters of pulse width 180 fs, wavelength 800 nm, and laser energy density 0.05 J / cm 2 , pulse frequency 1kHz, focused laser beam diameter 25 µm, immediately after completion transferred to nitrogen and oxygen (volume ratio 4:1) environment for 200℃ treatment for 6 h, then immediately secondary water quenching, and then purified water ultrasonic cleaning for 15 min, to obtain a surface micro-nano structure 5 containing a brick-like structure 12 and a bump structure 13; the needle body was preheated to 90℃, and a standard tip structure 1 and a standard blunt end structure 2 were prepared by CNC lathe cutting, and then ultrasonic cleaning was carried out in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then purified water ultrasonic cleaning for 15 min; the middle needle body B was fixed, and the two end structures A were anodized at 45V for 3 min, in which the ultrasonic type was CNC lathe cutting to prepare annular grooves 7 on the basis of anodizing, to obtain ultrasonic tip structure 3 and ultrasonic blunt end structure 4; finally, a smooth blunt structure 8 of the needle tip was prepared by fine grinding, and then purified water ultrasonic cleaning was carried out for 15 min to obtain a visualized anti-adhesion drag reduction and damage-free tunnel needle.
[0052] Example 5
[0053] Stainless steel material was selected, coarsely ground, heated to 850℃ and maintained for 3 min, quenched in water, placed in a 650℃ environment for 30 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; preheated to 40℃, and then the middle needle body B was subjected to three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser, with laser parameters of pulse width 350 fs, wavelength 257 nm, and laser energy density 0.11 J / cm 2, pulse frequency 250kHz, focused laser beam diameter 25 µm, immediately after completion transferred to nitrogen and oxygen (volume ratio 5:1) environment for 300℃ treatment for 2 h, then immediately secondary water quenching, and then purified water ultrasonic cleaning for 15 min, to obtain a surface micro-nano structure 5 containing a brick-like structure 12 and a bump structure 13; the needle body was preheated to 65℃, and a standard tip structure 1 and a standard blunt end structure 2 were prepared by CNC lathe cutting, and then ultrasonic cleaning was carried out in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then purified water ultrasonic cleaning for 15 min; the middle needle body B was fixed, and the two end structures A were anodized at 50V for 2 min, in which the ultrasonic type was CNC lathe cutting to prepare annular grooves 7 on the basis of anodizing, to obtain ultrasonic tip structure 3 and ultrasonic blunt end structure 4; finally, the needle tip smooth blunt structure 8 was prepared by fine grinding, and then purified water ultrasonic cleaning was carried out for 15 min, to obtain a visualized anti-adhesion drag reduction and damage-free tunnel needle.
[0054] Comparative Example 1
[0055] Stainless steel material was selected, coarsely ground, heated to 850℃ and maintained for 3 min, water quenched, placed in a 550℃ environment for 45 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; it was preheated to 65℃, and immediately transferred to a nitrogen and oxygen (volume ratio 4:1) environment for 200℃ treatment for 6 h, followed by a second water quenching, and then ultrasonically cleaned with purified water for 15 min; the needle body was preheated to 65℃, and a standard tip structure 1 and a standard blunt end structure 2 were prepared by CNC lathe cutting, and then ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the middle needle body B was fixed, and the two end structures A were anodized at a voltage of 50V for 2 min, wherein the ultrasonic type is subjected to CNC lathe cutting processing on the basis of anodizing to prepare an annular groove 7, thereby obtaining an ultrasonic tip structure 3 and an ultrasonic blunt end structure 4; finally, a needle tip smooth blunt structure 8 is prepared by fine grinding, and then ultrasonic cleaning with purified water for 15 min is performed.
[0056] Comparative Example 2
[0057] Stainless steel material was selected, coarsely ground, heated to 850℃ and maintained for 3 min, quenched in water, placed in a 550℃ environment for 45 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; preheated to 65℃, and then the middle needle body B was subjected to three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser, with laser parameters of pulse width 164 fs, wavelength 780 nm, and laser energy density 1.32 J / cm 2 , pulse frequency 1kHz, focused laser beam diameter 25 µm, immediately after completion transferred to nitrogen and oxygen (volume ratio 4:1) environment for 200 ℃ treatment for 6 h, then immediately secondary water quenching, and then purified water ultrasonic cleaning for 15 min, to obtain a surface micro-nano structure 5 containing a brick-like structure 12 and a bump structure 13; the needle body was preheated to 65 ℃, and a standard tip structure 1 and a standard blunt end structure 2 were prepared by CNC lathe cutting, and then ultrasonic cleaning was carried out in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then purified water ultrasonic cleaning was carried out for 15 min; the middle needle body B was fixed, and the two end structures A were anodized at 50 V for 2 min; finally, the needle tip smooth blunt structure 8 was prepared by fine grinding, and then purified water ultrasonic cleaning was carried out for 15 min.
[0058] Comparative Example 3
[0059] Stainless steel material was selected, coarsely ground, heated to 850℃ and maintained for 3 min, quenched in water, placed in a 550℃ environment for 45 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; preheated to 65℃, and then the middle needle body B was subjected to three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser, with laser parameters of pulse width 164 fs, wavelength 780 nm, and laser energy density 1.32 J / cm 2, pulse frequency 1kHz, focused laser beam diameter 25 µm, immediately after completion transferred to nitrogen and oxygen (volume ratio 4:1) environment for 200 ℃ treatment for 6 h, then immediately secondary water quenching, and then purified water ultrasonic cleaning for 15 min, to obtain a surface micro-nano structure 5 containing a brick-like structure 12 and a bump structure 13; the needle body is preheated to 65 ℃, and CNC lathe cutting process is used to prepare the tip ordinary structure and the standard blunt end structure 2, and then ultrasonic cleaning is carried out in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then purified water ultrasonic cleaning for 15 min; the middle needle body B is fixed, and the two end structures A are anodized at 50V for 2 min, in which the ultrasonic type is CNC lathe cutting process based on anodization to prepare annular grooves 7, to obtain the ultrasonic tip ordinary structure and ultrasonic blunt end structure 4; finally, the needle tip smooth blunt structure 8 is prepared by fine grinding process, and then purified water ultrasonic cleaning for 15 min.
[0060] Comparative Example 4
[0061] Stainless steel material was selected, coarsely ground, heated to 850℃ and maintained for 3 min, quenched in water, placed in a 550℃ environment for 45 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; preheated to 65℃, and then the middle needle body B was subjected to three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser, with laser parameters of pulse width 164 fs, wavelength 780 nm, and laser energy density 1.32 J / cm 2 , pulse frequency 1kHz, focused laser beam diameter 25 µm, immediately after completion transferred to nitrogen and oxygen (volume ratio 4:1) environment for 200 ℃ treatment for 6 h, then immediately secondary water quenching, and then purified water ultrasonic cleaning for 15 min, to obtain a surface micro-nano structure 5 containing a brick-like structure 12 and a bump structure 13; the needle body was preheated to 65 ℃, and a standard tip structure 1 and a standard blunt end structure 2 were prepared by CNC lathe cutting, and then ultrasonic cleaning was carried out in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then purified water ultrasonic cleaning was carried out for 15 min; the middle needle body B was fixed, and the two end structures A were anodized at 50 V for 2 min, among which the ultrasonic type was CNC lathe cutting on the basis of anodization to prepare an annular groove 7, to obtain an ultrasonic tip structure 3 and an ultrasonic blunt end structure 4; finally purified water ultrasonic cleaning was carried out for 15 min.
[0062] Comparative Example 5
[0063] Stainless steel material was selected, coarsely ground, heated to 200℃ and maintained for 0.5 min, water quenched, placed in a 200℃ environment for 10 min, cooled, and finely ground to obtain a tunnel needle matrix; the tunnel needle matrix was rinsed with flowing purified water for 5 min, ultrasonically cleaned in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then ultrasonically cleaned with purified water for 15 min; the surface was treated with cold atmospheric pressure plasma and blown dry with clean air; it was preheated to 30℃, and then the middle needle body B was subjected to three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser, with laser parameters of pulse width 5 fs, wavelength 100 nm, and laser energy density 0.01 J / cm 2 , pulse frequency 0.01 kHz, focused laser beam diameter 25 µm, immediately after completion transferred to nitrogen and oxygen (volume ratio 1:1) environment for 50 ℃ treatment for 1 h, then immediately secondary water quenching, and then purified water ultrasonic cleaning for 15 min, to obtain a surface micro-nano structure 5 containing a brick-like structure 12 and a bump structure 13; the needle body was preheated to 35 ℃, and a standard tip structure 1 and a standard blunt end structure 2 were prepared by CNC lathe cutting, and then ultrasonic cleaning was carried out in a mixed solution of anhydrous ethanol and acetone with a volume ratio of 1:1 for 15 min, and then purified water ultrasonic cleaning was carried out for 15 min; the middle needle body B was fixed, and the structures A at both ends were anodized at 25 V for 0.1 min, in which the ultrasonic type was CNC lathe cutting on the basis of anodization to prepare an annular groove 7, to obtain an ultrasonic tip structure 3 and an ultrasonic blunt end structure 4; finally, a smooth blunt structure 8 of the needle tip was prepared by fine grinding, and then purified water ultrasonic cleaning was carried out for 15 min.
[0064] The present invention adopts the following method to detect the visual anti-adhesion drag reduction and damage-free tunnel needle:
[0065] 1. Animal test: Animals were used for hydrophobicity test, drag reduction test and ultrasonic imaging test. Animal information: 6 male, SPF grade, 3 months old, weighing 2.5±0.5 kg, healthy New Zealand white rabbits, fed with standard pellets, free drinking water, single caged, and fed for 1 week under constant temperature and humidity conditions.
[0066] (1) Anti-adhesion test: Animals were selected as test subjects, and Examples 1-5 and Comparative Examples 1-5, each with a length of 130 mm, were selected for testing. The tunnel length was 5 cm, and the doctors, operation methods, and environment were all the same. The anti-adhesion property was tested by visual observation and the quality difference method. Visual observation is to observe the tunnel needle under indoor daylight with normal vision or corrected vision to observe the degree of body fluid on its surface. According to the observation results, the degree is divided into three levels: poor, general, and good. Among them, poor means obvious body fluid, and good means almost no body fluid; the quality difference method is to determine the content of the substance attached to the surface of the tunnel needle by measuring and calculating the quality difference before and after the use of the tunnel needle. The larger the quality difference, the more the substance content attached to the tunnel needle, which means the worse the anti-adhesion property.
[0067] (2) Drag reduction test: Animals were selected as test subjects, and Examples 1-5 and Comparative Examples 1-5, each with a length of 130 mm, were selected for testing. The tunnel length was 5 cm, and the doctors, operation methods, and environment were all the same. The test was conducted using a resistance testing machine, and the average value of the maximum resistance value was taken for 3 measurements.
[0068] (3) Ultrasound development detection: Animals were selected as test subjects, and Examples 1-5 and Comparative Examples 1-5, each with a length of 130 mm, were selected for testing. The tunnel length was 5 cm, and the doctors, operation methods, and environment were all the same. Ultrasound coupling agent was applied to the skin surface where the tunnel was located, and a portable ultrasonic diagnostic instrument was used to detect the tip of the tunnel needle and observe the development.
[0069] 2. Clinical trial: 210 patients who needed PICC were selected for a multicenter, prospective, randomized controlled clinical study and randomly divided into a control group and a study group. The patients in the control group used a traditional tunnel needle to establish a tunnel, and the patients in the study group used the visualized anti-adhesion, drag-reducing and injury-free tunnel needle prepared in Example 1 to establish a tunnel. The first puncture success rate, total complication rate, catheter fall-off rate, accidental injury rate, and the operator's praise rate for the actual use of the tunnel needle were followed up in the two groups of patients.
[0070] The effects of the visualized anti-adhesion, drag-reducing and injury-free tunnel needle were observed according to the above methods, and the results are shown in Tables 1-4.
[0071] Table 1 Animal test anti-adhesion test results
[0072]
[0073] Table 2 Animal test drag reduction test results
[0074]
[0075] Table 3 Animal experiment observation and development status
[0076]
[0077] Table 4 Clinical trial effect results
[0078]
[0079] As shown in Table 1, tunnel needles without laser treatment or inappropriate technical parameters can cause body fluid adhesion, which may affect the safety of use. Adhesion can also be caused by not making a double-stage gradient structure and not making a smooth blunt structure at the tip of the needle. The visualized anti-adhesion drag reduction and injury-free tunnel needle has good anti-adhesion properties. As shown in Table 2, not making laser treatment, not making a double-stage gradient structure, not making a smooth blunt structure at the tip of the needle, and not meeting the requirements of the preparation process parameters will cause increased resistance to puncture or tunnel establishment, which may increase the incidence of complications. As shown in Table 3, the visualized anti-adhesion drag reduction and injury-free tunnel needle is clearly visible under ultrasound, has good ultrasound visibility, and can improve surgical safety. As shown in Table 4, the visualized anti-adhesion drag reduction and injury-free tunnel needle can improve the first puncture success rate, reduce the incidence of complications, reduce the incidence of catheter detachment, reduce the incidence of accidental injuries, and reduce the difficulty of surgical operation, and has been widely praised.
[0080] The results show that the visualized anti-adhesion, drag-reducing and injury-free tunnel needle designed in the present invention has good properties and clinical application value.
[0081] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention can be made, and any changes that can be thought of by those skilled in the art should be within the scope of protection of the present invention.
Claims
1. A visual anti-adhesion drag-reducing and injury-free tunnel needle, characterized in that: The tunnel needle is composed of a straight solid stainless steel body without any other connecting parts, with a total length of 50-250mm, divided into a middle needle body and two end structures, the middle needle body and the two end structures are connected and transitioned by a gentle curved surface, and can be divided into several specifications according to the total length of the tunnel needle; the middle needle body belongs to the main part of the tunnel needle, with a diameter of 1.8-2.2mm, a length of 30-240mm, a cylindrical shape, and a micro-nano level rib structure on the surface; the rib structure is composed of a periodically cross-arranged micro-nano level brick-like structure and a convex point structure, with a brick-like structure The brick-like structure and three convex point structures are arranged and combined as a period, the brick-like structure and the convex point structure are in contact with each other up and down, left and right, and are closely connected, and the overall height of the two structures is 30-60μm, which can achieve anti-adhesion and reduce the use resistance at the same time; the brick-like structure is stacked by a rectangular block at the bottom and a tetrahedron at the top, the length and width of the upper and lower bottom surfaces of the rectangular block are consistent with the length and width of the lower bottom surface of the tetrahedron, both of which are 90-180μm, and the width is 30-60μm, and the height of the rectangular block is consistent with the height of the tetrahedron, both of which are 15-30μm; the convex point structure is composed of a circular frustum at the bottom The diameter of the upper base of the truncated cone is consistent with that of the hemispherical body, both of which are 15-25μm; the structures at both ends belong to the functional structures of the tunnel needle, both of which have rough surfaces, with a total length of 13-17mm, and both of which have smooth and blunt structures at the very end, which can automatically avoid blood vessels, nerves and other tissues to avoid accidental injuries; the roughness of the rough surface is 2-50μm; the smooth and blunt structure is a spherical structure with a radius of 0.30-1.2mm; according to the characteristics of the structures at both ends, it is divided into standard type and ultrasonic type; the difference between the standard type and the ultrasonic type is that the two ends of the ultrasonic type The end structure has been roughened, and with the help of an external ultrasonic device, the image is clearer and the visualization is more significant; the roughening treatment is to set a total of 5-12 annular grooves, and the annular grooves are transitioned by a gentle curved surface; the cross-section of the annular groove is a semicircle, the distance between the centers of the semicircles is 0.5-0.7mm, and the radius of the semicircle is 0.08-0.12mm; the standard type is divided into type I and type II, and the ultrasonic type is divided into type III and type IV; the overall structure of type I and type III is divided into a tip, a middle needle body and a blunt end from left to right, and the overall structure of type II and type IV is divided into a tip, a middle needle body and a tip from left to right; The tip is a double-stage gradient structure, and the double-stage gradient represents that the tip is composed of a primary gradient structure and a secondary gradient structure, wherein the primary gradient structure has a smaller diameter than the secondary gradient structure, and the secondary gradient structure has a smaller diameter than the middle needle body, the primary gradient structure has a diameter of 0.7-1.1 mm, and the secondary gradient structure has a diameter of 1.3-1.7 mm, and each level is transitioned by a spherical arc surface structure; the spherical arc surface structure is 0.5-1.5 mm long, which can increase the smoothness of the catheter connection and increase the friction between the catheter and the catheter, prevent the catheter from slipping, and promote the establishment of the tunnel; the blunt end is a spherical structure with a radius of 1.8-2.2 mm; The preparation method comprises the following steps: (1) Preparation of tunnel needle substrate: Select stainless steel material, perform rough grinding, heating, water quenching, tempering, cooling, and fine grinding; (2) Preparation of surface micro-nanostructure: Select the tunnel needle substrate, rinse with flowing purified water for 5 min, ultrasonically clean with mixed organic solution for 15 min, and ultrasonically clean with purified water for 15 min; treat the surface with cold atmospheric pressure plasma and blow dry with clean air; preheat, perform three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser on the middle needle body, and immediately transfer it to a nitrogen and oxygen environment for high temperature treatment, followed by secondary water quenching, and then ultrasonic cleaning with purified water; (3) Preparation of the tip double-stage gradient structure and blunt-end structure: preheat the needle body, cut it on a CNC lathe, and then ultrasonically clean it with a mixed organic solution for 15 min and with purified water for 15 min; (4) Special treatment of the two end structures: fix the middle needle body and perform anodizing on the two end structures; ultrasonic type performs CNC lathe cutting on the basis of anodizing to prepare annular grooves; (5) Preparation of visualized anti-adhesion, drag-reducing and damage-free tunnel needle: The needle tip is made into a smooth and blunt structure through fine grinding, and then ultrasonically cleaned with purified water to obtain a tunnel needle.
2. The visualized anti-adhesion drag-reducing and injury-free tunnel needle according to claim 1 is characterized in that: The tunnel needle is composed of a straight solid stainless steel body without any other connecting parts, with a total length of 50-250mm, and is divided into a middle needle body and two end structures, and the middle needle body and the two end structures are connected and transitioned by a gentle curved surface; according to the characteristics of the two end structures of the tunnel needle, the tunnel needle is divided into a standard type and an ultrasonic type, wherein the standard type includes type I and type II, and the ultrasonic type includes type III and type IV; type I has one sharp end and one blunt end, type II has two sharp ends, type III has one sharp end and one blunt end after roughening, and type IV has two The tip after roughening treatment; Type I, Type II, Type III and Type IV include but are not limited to Fr6-50, Fr6-60, Fr6-70, Fr6-80, Fr6-90, Fr6-100, Fr6-110, Fr6-120, Fr6-130, Fr6-140, Fr6-150, Fr6-160, Fr6-170, Fr6-180, Fr6-190, Fr6-200, Fr6-210, Fr6-220 and Fr6-230.
3. The visualized anti-adhesion drag-reducing and injury-free tunnel needle according to claim 1 is characterized in that: The rib structure is composed of a periodically cross-arranged micro-nano-scale brick-like structure and a micro-nano-scale convex point structure; the brick-like structure is composed of a lower rectangular block and an upper tetrahedron stacked together, the length, width and height of the lower rectangular block are 90-180μm, 30-60μm and 15-30μm respectively; the length and width of the upper bottom surface of the tetrahedron are 45-85μm and 10-20μm respectively; the height of the tetrahedron is 15-30μm; the convex point structure is composed of a lower truncated cone and an upper hemisphere-like stacked together, the diameter of the lower bottom surface of the lower truncated cone is 30-60μm.
4. The visualized anti-adhesion drag-reducing and injury-free tunnel needle according to claim 1, characterized in that: The roughening treatment is to set 5-12 annular grooves on the two end structures; the cross-section of the annular groove is a semicircle, the distance between the centers of the semicircles is 0.5-0.7mm, the radius of the semicircle is 0.08-0.12mm, the distance between the annular grooves is 0.34-0.46mm, and the distance from the center of the outermost annular groove to the end of the two end structures is 1.5-2.5mm.
5. A method for preparing a visualized anti-adhesion drag-reducing and injury-free tunnel needle as claimed in any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) Preparation of tunnel needle substrate: Select stainless steel material, perform rough grinding, heating, water quenching, tempering, cooling, and fine grinding; (2) Preparation of surface micro-nanostructure: Select the tunnel needle substrate, rinse with flowing purified water for 5 min, ultrasonically clean with mixed organic solution for 15 min, and ultrasonically clean with purified water for 15 min; treat the surface with cold atmospheric pressure plasma and blow dry with clean air; preheat, perform three-dimensional ultrasonic nitrogen jet-assisted femtosecond laser on the middle needle body, and immediately transfer it to a nitrogen and oxygen environment for high temperature treatment, followed by secondary water quenching, and then ultrasonic cleaning with purified water; (3) Preparation of the tip double-stage gradient structure and blunt-end structure: preheat the needle body, cut it on a CNC lathe, and then ultrasonically clean it with a mixed organic solution for 15 min and with purified water for 15 min; (4) Special treatment of the two end structures: fix the middle needle body and perform anodizing on the two end structures; ultrasonic type performs CNC lathe cutting on the basis of anodizing to prepare annular grooves; (5) Preparation of visualized anti-adhesion, drag-reducing and damage-free tunnel needle: The needle tip is made into a smooth and blunt structure through fine grinding, and then ultrasonically cleaned with purified water to obtain a tunnel needle.
6. The method for preparing the visualized anti-adhesion drag-reducing and injury-free tunnel needle according to claim 5, characterized in that: In step (1), the stainless steel material is one of 06Cr19Ni10, 06Cr17Ni12Mo2, 00Cr19Ni10, and 00Cr17Ni14Mo2; the heating temperature is 700-1000°C, and the duration is 1-5 min; the tempering temperature is 450-650°C, and the duration is 30-60 min.
7. The method for preparing the visualized anti-adhesion drag-reducing and injury-free tunnel needle according to claim 5, characterized in that: The mixed organic solution in step (2) is an anhydrous ethanol and acetone solution in a volume ratio of 1:1, and the ultrasonic cleaning time is 15 minutes; the gas used for the cold atmospheric pressure plasma treatment is one or both of argon and helium; the preheating temperature is 40-90°C; the three-dimensional ultrasonic nitrogen jet combines the ultrasonic system, the nitrogen emission system and the three-dimensional motion system to reduce the fall and adhesion of the laser ablation products generated by the femtosecond laser in the laser working area on the surface of the tunnel needle, so as to improve the laser processing efficiency and the microstructure quality; the femtosecond laser parameters are a pulse width of 25-350fs, a wavelength of 250-800nm, and a laser energy density of 0.05-1.5J / cm 2 , a pulse frequency of 1-250kHz, a focused laser beam diameter of 25μm; the nitrogen-oxygen environment is an environment formed by a mixture of nitrogen and oxygen in a volume ratio of 3-5:1, a high-temperature treatment temperature of 100-300°C, and a duration of 2-10h.
8. The method for preparing the visualized anti-adhesion drag-reducing and injury-free tunnel needle according to claim 5, characterized in that: In step (3), the preheating temperature is 40-90° C., and the ultrasonic cleaning time is 15 min. The mixed organic solution is an anhydrous ethanol and acetone solution with a volume ratio of 1:1, and the ultrasonic cleaning time is 15 min.
9. The method for preparing the visualized anti-adhesion drag-reducing and injury-free tunnel needle according to claim 5, characterized in that: The anodic oxidation in step (4) has an oxidation time of 1-3 minutes and a voltage of 45-65V.
Citation Information
Patent Citations
Tools and usage methods for subcutaneous tunnel creation during tunnel-type PICC placement
CN110960298B
Subcutaneous tunnel building assembly for tunnel type PICC (peripherally inserted central catheter)
CN214128714U
Dual-purpose tunnel needle for axillary vein puncture
CN215386541U
Hyperechoic stimulating block needle
US20070179508A1