Titanium and titanium alloy watch case casting and preparation method

By using a combination of a vacuum fast induction melting furnace and a zirconium fiber ceramic crucible in the production of titanium and titanium alloy castings, the power of the smelting power is increased to achieve rapid charging, and the internal defects and low production efficiency of titanium and titanium alloy castings are solved, and the problem of internal defects and low production efficiency of titanium and titanium alloy castings is achieved. Efficient and low-cost casting manufacturing.

CN118513509BActive Publication Date: 2024-11-22LUOYANG SUNRUI TI PRECISION CASTING +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410989125.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-22
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

There are many internal defects, low production efficiency and high cost in the production of existing titanium and titanium alloy castings, especially in the mass production of small titanium and titanium alloy castings, which are difficult to achieve efficient and low-cost manufacturing.

Method used

Use a vacuum fast induction melting furnace and bottomless zirconium fiber ceramic crucible to increase the power of the melting power to 200~250kw. Through gravity, the ceramic shell is quickly filled with gravity to realize the casting of small titanium and titanium alloy castings, avoid internal defects and improve production. efficiency.

Benefits of technology

Effectively solve the problems of difficulty in filling, low production efficiency and high production costs of small titanium and titanium alloy castings, and achieve high quality and large-scale rapid production of titanium and titanium alloy castings, reducing production costs, and ensuring the internal castings. quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118513509B_ABST
    Figure CN118513509B_ABST
Patent Text Reader

Abstract

The present invention provides a titanium and titanium alloy watch case casting and a preparation method, the method comprising the following steps: S1, processing titanium and titanium alloy ingots to obtain titanium and titanium alloy round ingots; S2, preparing wax molds and mold frames, welding the wax molds on the mold frames; then bonding the mold frames and zirconium fiber ceramic crucibles together; preparing the mold shell surface layer and the mold shell back layer of the mold frame and the zirconium fiber ceramic crucible; then dewaxing treatment, and finally roasting to prepare a ceramic mold shell; S3, placing the titanium and titanium alloy round ingots in the zirconium fiber ceramic crucible, placing the ceramic mold shell with the titanium and titanium alloy round ingots in a vacuum induction rapid melting furnace for smelting, increasing the power of the smelting power supply to 200-250kw, forming titanium and titanium alloy castings; stopping the furnace for cooling to obtain titanium and titanium alloy watch case castings. The preparation method of the titanium and titanium alloy watch case castings of the present invention can avoid defects inside the titanium and titanium alloy castings, improve production efficiency, and reduce production costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of titanium and titanium alloy casting, and in particular to a titanium and titanium alloy watch case casting and a preparation method thereof. Background Art

[0002] At present, titanium alloy watch cases are mainly formed by forging + machining, powder metallurgy and vacuum casting. Casting + machining is costly and inefficient, which seriously affects the mass production of titanium alloy watch cases. Powder metallurgy methods have defects such as difficult to control deformation and shrinkage and many internal holes. Titanium and titanium alloy castings are generally cast in vacuum consumable arc shell furnaces and water-cooled copper crucible vacuum rapid induction melting furnaces. Vacuum consumable electrode arc shell furnaces are suitable for large titanium alloy castings. At the same time, due to the difficulty in preheating the mold shell, this furnace is suitable for pouring thick and large titanium and titanium alloy castings. However, for thin-walled small titanium and titanium alloy castings, it is very easy to have mold shell cracks, incomplete filling, solidification cracking, surface cold shut, low production efficiency, high production cost and other problems. Although the vacuum rapid induction melting furnace has a high alloy superheat and is suitable for the preparation of small titanium and titanium alloy castings, the single melting volume is small and its efficiency is low, and it cannot meet the production of large batches of titanium and titanium alloy castings efficiently and at low cost. In addition, both the vacuum consumable electrode arc shell furnace and the vacuum rapid induction melting furnace have many internal defects, low production efficiency, high cost and other problems.

[0003] At present, the structural parts of civil products are pursuing integration, high precision, light weight and low cost, and the requirements for product quality are getting higher and higher. Titanium and titanium alloys have gradually been used in sports, medical and electronic products due to their excellent performance, but their low production efficiency and high price have restricted their wider application in these fields. With the technological progress and development of civil electronics and wearable products, small titanium alloy castings are increasingly used in electronic products and wearable products, and the demand is increasing. Rapid and low-cost manufacturing of titanium and titanium alloy castings is the trend of future development.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a titanium and titanium alloy watch case casting and a preparation method thereof, so as to solve the problems of many internal defects, low production efficiency and high cost of small and medium-sized titanium and titanium alloy castings in the prior art.

[0006] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0007] A method for preparing titanium and titanium alloy watch case castings, the preparation method comprising the following steps:

[0008] S1. Preparation of titanium and titanium alloy ingots: processing titanium and titanium alloy ingots to obtain titanium and titanium alloy ingots;

[0009] S2, shell preparation: prepare wax mold and mold frame, weld the wax mold assembly to the mold frame; then bond the mold frame and zirconium fiber ceramic crucible together; prepare the shell surface layer and shell back layer of the mold frame and zirconium fiber ceramic crucible; then dewax treatment, and finally roast to prepare a ceramic shell for casting;

[0010] S3, casting and molding: put the titanium and titanium alloy ingots in the zirconium fiber ceramic crucible, put the ceramic shell with the titanium and titanium alloy ingots in the vacuum induction rapid melting furnace for melting, increase the power of the melting power supply to 200~250kw, and mold the titanium and titanium alloy castings; then stop the furnace for cooling to obtain the cast titanium and titanium alloy watch case castings.

[0011] The preparation method of titanium and titanium alloy watch case castings described in the present invention uses a vacuum rapid induction melting furnace in conjunction with a bottomless zirconium fiber ceramic crucible to increase the power of the melting power supply to 200-250 kW, so that the titanium and titanium alloy ingots can be quickly melted within 1 minute, and the ceramic mold shell can be quickly filled under the action of gravity to achieve the casting of small titanium and titanium alloy castings, thereby avoiding defects inside the titanium and titanium alloy castings, improving production efficiency, and reducing production costs.

[0012] Further, step S3 includes the following steps:

[0013] S31, shell loading: taking out the fired ceramic shell, placing the titanium and titanium alloy round ingots in the zirconium fiber ceramic crucible, placing the ceramic shell loaded with the titanium and titanium alloy round ingots in the cavity of the vacuum induction rapid melting furnace, and sealing;

[0014] S32, vacuuming: starting the vacuum pump equipment of the sealed vacuum induction rapid melting furnace to vacuumize the cavity;

[0015] S33, argon backfilling: filling the vacuum chamber with argon;

[0016] S34, heating and melting: start the melting power supply, increase the power of the melting power supply to 200-250kw, and the molten titanium and titanium alloy are quickly filled into the ceramic shell under the action of gravity to form titanium and titanium alloy castings;

[0017] S35. Shut down the furnace for cooling: turn off the smelting power supply, and let the ceramic shell stand in the furnace chamber for 2 to 4 minutes to cool. When the titanium and titanium alloy melt in the ceramic shell are completely solidified, take out the ceramic shell from the cavity, and when the ceramic shell cools to below 300°C, break the ceramic shell and take out the cast titanium alloy watch case casting.

[0018] Furthermore, step S1 specifically includes: subjecting the titanium and titanium alloy ingots to sizing, surface lathing, surface polishing, surface pickling and water washing, and then drying to prepare titanium and titanium alloy round ingots.

[0019] Furthermore, in step S1, the diameter of the titanium and titanium alloy ingot is 48-50 mm, and the length is 180-220 mm.

[0020] Furthermore, in step S1, an acid solution is used in the surface pickling treatment, and the acid solution includes water, nitric acid and hydrofluoric acid, and the weight ratio of water, nitric acid and hydrofluoric acid is 8:3:2. The surface pickling treatment time is 5 to 10 minutes.

[0021] Furthermore, in step S2, the calcination temperature is 950°C and the holding time is 4 hours.

[0022] Furthermore, in step S2, after preparing the wax mold and mold frame for forming the titanium alloy watch case, the prepared wax mold and mold frame are placed in a constant temperature and humidity workshop for a placement time of ≥ 4 hours. After the size of the wax mold and mold frame shrinks and stabilizes, the wax mold assembly is welded to the mold frame.

[0023] Furthermore, in step S32, the cavity is evacuated to make the vacuum degree in the cavity less than 0.9Pa.

[0024] Furthermore, in step S33, the vacuum chamber is filled with argon gas to control the chamber pressure to 20000-30000Pa.

[0025] In a second aspect of the present invention, a titanium and titanium alloy watch case casting is provided, wherein the titanium and titanium alloy watch case casting is prepared using the above-mentioned method for preparing the titanium and titanium alloy watch case casting.

[0026] The present invention provides a titanium and titanium alloy watch case casting and a preparation method. Compared with the prior art, the titanium and titanium alloy watch case casting and a preparation method of the present invention have the following beneficial effects:

[0027] The present invention discloses a titanium and titanium alloy watch case casting and a preparation method thereof. The method utilizes a vacuum rapid induction melting furnace in conjunction with a bottomless zirconium fiber ceramic crucible to increase the power of the melting power source to 200-250 kW, so that the titanium and titanium alloy ingots can be rapidly melted within 1 minute, and the ceramic mold shell can be rapidly filled under the action of gravity to realize the casting of small titanium and titanium alloy castings, thereby avoiding defects inside the titanium and titanium alloy castings and greatly improving the production efficiency of the titanium and titanium alloy castings; reducing the production cost of the titanium and titanium alloy castings, effectively ensuring the rapid mass production of the titanium and titanium alloy castings, and effectively solving the problems of difficult filling of small titanium and titanium alloy castings, low production efficiency and high production cost.

[0028] The titanium and titanium alloy watch case casting and preparation method described in the present invention can achieve the filling integrity of the titanium and titanium alloy casting with a wall thickness of less than 1mm due to the high mold shell temperature.

[0029] The titanium and titanium alloy watch case casting and preparation method described in the present invention are that the titanium and titanium alloy are filled into a mold immediately after melting, the alloy has a low superheat and a small solidification shrinkage tendency, and therefore the prepared titanium and titanium alloy casting has a good internal quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 A schematic diagram of a titanium alloy watch case casting according to an embodiment of the present invention;

[0031] Figure 2 A schematic diagram of a zirconium fiber ceramic crucible used in a method for preparing a titanium and titanium alloy watch case casting according to an embodiment of the present invention;

[0032] Figure 3 It is a schematic diagram of a method for preparing a titanium and titanium alloy watch case casting according to an embodiment of the present invention after casting of a medium-sized shell;

[0033] Figure 4 A schematic diagram of a vacuum rapid induction melting furnace used in a method for preparing titanium and titanium alloy watch case castings according to an embodiment of the present invention;

[0034] Figure 5 This is one of the structural schematic diagrams of a mold frame used in a method for preparing a titanium and titanium alloy watch case casting according to an embodiment of the present invention;

[0035] Figure 6 This is a second schematic diagram of the structure of a mold frame used in a method for preparing a titanium and titanium alloy watch case casting according to an embodiment of the present invention.

[0036] Description of reference numerals:

[0037] 1. Vacuum pump equipment; 2. Melting power supply; 3. Lifting cylinder; 4. Water-cooled volute; 5. Mold shell and crucible; 6. Induction coil; 7. Alloy material; 8. Quartz glass cover; 9. Tray; 10. Cavity; 11. Mold frame. DETAILED DESCRIPTION

[0038] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The descriptions of "first", "second", etc. mentioned in the embodiments of the present invention are only for descriptive purposes, and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0039] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.

[0040] like Figures 1 to 6 As shown, the present invention provides a method for preparing titanium and titanium alloy watch case castings, the preparation method comprising the following steps:

[0041] S1. Preparation of titanium and titanium alloy ingots: The titanium and titanium alloy ingots used in a vacuum induction rapid melting furnace are subjected to sizing, surface lathing, surface polishing, surface pickling and water washing, and then dried to prepare titanium and titanium alloy ingots;

[0042] S2, shell preparation: prepare wax molds and mold frames 11 for forming titanium and titanium alloy watch cases, weld the wax mold assembly to the mold frame 11; then use bonding wax to bond the mold frame 11 and the zirconium fiber ceramic crucible together; prepare the mold frame 11 and the zirconium fiber ceramic crucible for the shell surface layer and the shell back layer, and the number of layers is 5 and a half; dewax the prepared 5 and a half layers of ceramic shell to remove the wax inside the shell; and calcine the dewaxed shell to prepare a ceramic shell for casting;

[0043] S3, casting and molding: placing titanium and titanium alloy ingots in a zirconium fiber ceramic crucible, placing the ceramic shell containing the titanium and titanium alloy ingots in a vacuum induction rapid melting furnace for melting, increasing the power of the melting power supply 2 to 200-250kw to form titanium and titanium alloy castings; then stopping the furnace for cooling to obtain a casting-molded titanium alloy watch case casting.

[0044] Steps S1 to S3 are interrelated and inseparable. Through step S1, on the one hand, a round ingot of suitable size can be obtained to match with the zirconium fiber ceramic crucible, and on the other hand, it can be ensured that the surface of the titanium and titanium alloy round ingot is free of oxide scale and foreign matter; through step S2, the shell preparation is convenient for step S3 to form titanium and titanium alloy castings. The inner surface of the zirconium fiber ceramic crucible has a highly inert coating resistant to titanium liquid corrosion. The zirconium fiber ceramic crucible has high inertness and can react with titanium and titanium alloy liquid in a relatively short time without obvious chemical reaction, which effectively solves the problem of small titanium and titanium alloy castings using vacuum The problem of crucible corrosion in the rapid induction melting furnace is facilitated by step S3 for quickly preparing titanium and titanium alloy castings in a vacuum rapid induction melting furnace; by increasing the power of the smelting power supply 2 to 200-250 kW in step S3, the titanium and titanium alloy ingots can be melted within 1 minute. On the one hand, the reaction of the titanium and titanium alloy solution with the zirconium fiber ceramic crucible can be avoided in a short time, thereby avoiding defects inside the titanium and titanium alloy castings, thereby ensuring the quality of the titanium and titanium alloy castings; on the other hand, the production efficiency of titanium and titanium alloy castings is greatly improved; and the production cost of titanium and titanium alloy castings is reduced.

[0045] In summary, the present invention proposes a method for preparing titanium and titanium alloy watch case castings, which uses a zirconium fiber ceramic crucible in conjunction with a vacuum rapid induction melting furnace, first, to achieve rapid melting of a small amount of titanium and titanium alloys, and to quickly fill the ceramic mold shell under the action of gravity to achieve the casting of small titanium and titanium alloy castings; it can effectively solve the problems of difficult filling of small titanium and titanium alloy castings, low production efficiency, and high production cost, greatly improve the production efficiency of titanium and titanium alloy castings, reduce the production cost of titanium and titanium alloy castings, and effectively ensure the large-scale rapid production of titanium and titanium alloy castings; second, due to the high mold shell temperature, this method can achieve the filling integrity of titanium and titanium alloy castings with a wall thickness of less than 1mm; third, titanium and titanium alloys are filled after melting, the alloy superheat is low and the solidification shrinkage trend is small, so the prepared titanium and titanium alloy castings have good internal quality.

[0046] Specifically, the present invention proposes a method for preparing titanium and titanium alloy watch case castings, which is suitable for all titanium and titanium alloys. The present application does not specifically limit the material of titanium and titanium alloys, and can be pure titanium or ZTC4 titanium alloy, but is not limited thereto.

[0047] Specifically, Figure 4 As shown, the vacuum induction rapid melting furnace includes a vacuum pump device 1, a smelting power supply 2, a lifting cylinder 3, a water-cooled volute 4, an induction coil 6, a quartz glass cover 8, a tray 9 and a cavity 10. The mold shell and the crucible 5 are placed on the tray 9, the alloy material 7 is in the mold shell and the crucible 5, and the titanium and titanium alloy ingots are melted to form the alloy material 7.

[0048] Specifically, step S3 includes the following steps:

[0049] S31, shell loading: take out the fired ceramic shell, place the titanium and titanium alloy ingots in the zirconium fiber ceramic crucible, place the ceramic shell loaded with the titanium and titanium alloy ingots in the cavity 10 of the vacuum induction rapid melting furnace, and seal it;

[0050] S32, vacuuming: starting the vacuum pump device 1 of the sealed vacuum induction rapid melting furnace to vacuumize the cavity 10;

[0051] S33, argon backfilling: filling the vacuum chamber 10 with argon;

[0052] S34, heating and melting: starting the melting power source 2, increasing the power of the melting power source 2 to 200-250 kW, and rapidly filling the molten titanium and titanium alloy into the ceramic shell under the action of gravity to form titanium and titanium alloy castings;

[0053] S35, stop the furnace for cooling: turn off the smelting power supply 2, let the ceramic shell stand in the furnace chamber for 2 to 4 minutes to cool, wait for the titanium and titanium alloy melt in the ceramic shell to completely solidify, take out the ceramic shell from the furnace chamber, wait for the ceramic shell to cool to below 300°C, break the ceramic shell, and take out the cast titanium alloy watch case casting.

[0054] Steps S31 to S35 are interrelated and inseparable. The argon backfilling in step S33 can prevent the titanium and titanium alloy ingots from splashing during the melting process; the power of the smelting power supply 2 is increased to 200-250 kW by step S34, so that the titanium and titanium alloy ingots can be melted within 1 minute. On the one hand, the reaction of the titanium and titanium alloy solution with the zirconium fiber ceramic crucible can be avoided in a short time, thereby avoiding defects in the titanium and titanium alloy castings and ensuring the quality of the castings; on the other hand, the production efficiency of titanium and titanium alloy castings is greatly improved; and the production cost of titanium and titanium alloy castings is reduced.

[0055] Specifically, step S31 is as follows: take out the sintered ceramic shell, place the titanium and titanium alloy ingots in the zirconium fiber ceramic crucible, and avoid excessive collision between the titanium and titanium alloy ingots and the zirconium fiber ceramic crucible during the placement process to prevent impurities from entering the shell; place the ceramic shell with the titanium and titanium alloy ingots on the tray 9 of the vacuum induction rapid melting furnace, start the lifting switch of the vacuum induction rapid melting furnace, and lift the cylinder 3 to send the ceramic shell into the cavity 10 of the vacuum induction rapid melting furnace for sealing.

[0056] The tray 9 and the cavity 10 fit tightly together to ensure good sealing and prevent air leakage.

[0057] Specifically, in step S2, the calcination temperature is 950°C and the holding time is 4 hours.

[0058] Specifically, in step S1, the diameter of the titanium and titanium alloy ingot is 48-50 mm, and the length is 180-220 mm.

[0059] Specifically, in step S1, an acid solution is used during the surface pickling treatment, and the acid solution includes water, nitric acid and hydrofluoric acid, the weight ratio of water, nitric acid and hydrofluoric acid is 8:3:2, the content of nitric acid in the nitric acid is 65-68%, the content of hydrofluoric acid in the hydrofluoric acid is 40%, and the surface pickling treatment time is 5-10 minutes.

[0060] Specifically, in step S1, during the surface polishing process, 0.2 mm is removed on one side.

[0061] Specifically, in step S2, after preparing the wax mold and mold frame 11 for forming the titanium alloy watch case, the prepared wax mold and mold frame 11 are placed in a constant temperature and humidity workshop for a placement time of ≥4 hours. After the size of the wax mold and mold frame 11 shrinks and stabilizes, the wax mold assembly is welded to the mold frame 11.

[0062] Specifically, in step S32 , the cavity 10 is evacuated to make the vacuum degree in the cavity 10 less than 0.9 Pa.

[0063] Specifically, in step S33, the vacuum chamber 10 is filled with argon gas, and the pressure of the chamber 10 is controlled to be 20000-30000Pa.

[0064] This setting can prevent alloy splashing during the melting process of titanium and titanium alloy ingots.

[0065] The raw materials of the zirconium fiber ceramic crucible of the present invention include zirconium oxide ceramic fiber, a dispersant and a binder. The inner surface of the zirconium fiber ceramic crucible has a highly inert coating resistant to titanium liquid corrosion.

[0066] There is no limitation on the specific types of dispersants and binders.

[0067] There is no specific limitation on the preparation method of the zirconium fiber ceramic crucible, and the preparation method commonly used in the prior art can also be used by the preparation method listed below. The preparation method of the zirconium fiber ceramic crucible of the present invention comprises the following steps:

[0068] (1) Preparing a zirconia ceramic fiber crucible using zirconia ceramic fiber, a dispersant and a binder;

[0069] (2) A highly inert titanium liquid corrosion-resistant coating is coated on the inside of a zirconia ceramic fiber crucible to obtain a ceramic crucible suitable for casting titanium and titanium alloys in a fast melting furnace.

[0070] The present invention places a titanium or titanium alloy round ingot with a diameter of 48-50 mm and a length of 180-220 mm into a bottomless zirconium fiber ceramic crucible, and uses a 200-250 kw high-power vacuum induction rapid melting furnace to rapidly melt the alloy within 1 minute. The melted titanium or titanium alloy liquid is filled into a high-temperature preheated mold cavity 10 under the action of gravity, and a small-sized high-quality titanium or titanium alloy casting is rapidly prepared. The molding method promotes the development of low-cost, high-quality titanium or titanium alloy castings, and the method realizes rapid and low-cost manufacturing of small-sized titanium or titanium alloy castings.

[0071] Example 1

[0072] This embodiment provides a method for preparing a titanium alloy watch case casting, the preparation method comprising the following steps:

[0073] S1. Titanium alloy round ingot: The titanium alloy ingot used in the vacuum induction rapid melting furnace is subjected to sizing treatment, surface lathing treatment, surface polishing treatment, surface pickling treatment and water washing treatment, and then dried to prepare a titanium alloy round ingot;

[0074] S2, shell preparation: prepare a wax mold and a mold frame 11 for forming a titanium alloy watch case, and weld the wax mold assembly to the mold frame 11; then use bonding wax to bond the mold frame 11 and the zirconium fiber ceramic crucible together; prepare the mold frame 11 and the zirconium fiber ceramic crucible for the shell surface layer and the shell back layer, and the number of layers is 5 and a half; dewax the prepared 5 and a half layers of ceramic shell to remove the wax inside the shell; and calcine the dewaxed shell to prepare a ceramic shell for casting;

[0075] S3, casting and molding: placing a titanium alloy ingot in a zirconium fiber ceramic crucible, placing the ceramic shell containing the titanium alloy ingot in a vacuum induction rapid melting furnace for melting, increasing the power of the melting power source 2 to 215kw to form a titanium alloy casting; then stopping the furnace for cooling to obtain a casting-molded titanium alloy watch case casting.

[0076] Specifically, the material of the titanium alloy is ZTC4 titanium alloy.

[0077] Specifically, Figure 4 As shown, the vacuum induction rapid melting furnace includes a vacuum pump device 1, a smelting power supply 2, a lifting cylinder 3, a water-cooled volute 4, an induction coil 6, a quartz glass cover 8, a tray 9 and a cavity 10. The mold shell and the crucible 5 are placed on the tray 9, the alloy material 7 is in the mold shell and the crucible 5, and the titanium alloy ingot is melted to form the alloy material 7.

[0078] Specifically, step S3 includes the following steps:

[0079] S31, loading the mold shell into the furnace: taking out the fired ceramic mold shell, placing the titanium alloy round ingot in the zirconium fiber ceramic crucible, placing the ceramic mold shell loaded with the titanium alloy round ingot in the cavity 10 of the vacuum induction rapid melting furnace, and sealing it;

[0080] S32, vacuuming: starting the vacuum pump device 1 of the sealed vacuum induction rapid melting furnace to vacuumize the cavity 10;

[0081] S33, argon backfilling: filling the vacuum chamber 10 with argon;

[0082] S34, heating and melting: starting the melting power source 2, increasing the power of the melting power source 2 to 215 kW, and rapidly filling the molten titanium alloy into the ceramic shell under the action of gravity to form a titanium alloy casting;

[0083] S35, stop the furnace for cooling: turn off the smelting power 2, let the ceramic shell stand in the furnace chamber for 4 minutes to cool, wait for the titanium alloy melt in the ceramic shell to completely solidify, take out the ceramic shell from the furnace chamber, wait for the ceramic shell to cool to 290°C, break the ceramic shell, and take out the cast titanium alloy watch case casting.

[0084] Specifically, S31, loading the mold shell into the furnace: take out the fired ceramic mold shell, place the titanium alloy ingot in the zirconium fiber ceramic crucible, and avoid excessive collision between the titanium alloy ingot and the zirconium fiber ceramic crucible during the placement process to prevent impurities from entering the mold shell; place the ceramic mold shell with the titanium alloy ingot on the tray 9 of the vacuum induction rapid melting furnace, start the lifting switch of the vacuum induction rapid melting furnace, and lift the cylinder 3 to send the ceramic mold shell into the cavity 10 of the vacuum induction rapid melting furnace for sealing.

[0085] The tray 9 and the cavity 10 fit tightly together to ensure good sealing and prevent air leakage.

[0086] Specifically, in step S2, the calcination temperature is 950°C and the holding time is 4 hours.

[0087] Specifically, in step S1, the diameter of the titanium alloy ingot is 48.3 mm and the length is 210.5 mm.

[0088] Specifically, in step S1, an acid solution is used for the surface pickling treatment, and the acid solution includes water, nitric acid and hydrofluoric acid, and the weight ratio of water, nitric acid and hydrofluoric acid is 8:3:2. The content of nitric acid in the nitric acid is 68%, and the content of hydrofluoric acid in the hydrofluoric acid is 40%. The surface pickling treatment time is 5 minutes.

[0089] Specifically, in step S1, during the surface polishing process, 0.2 mm is removed on one side.

[0090] Specifically, in step S2, after preparing the wax mold and mold frame 11 for forming the titanium alloy watch case, the prepared wax mold and mold frame 11 are placed in a constant temperature and humidity workshop for 4 hours. After the size of the wax mold and mold frame 11 shrinks and stabilizes, the wax mold assembly is welded to the mold frame 11.

[0091] Specifically, in step S32 , the cavity 10 is evacuated to a vacuum level of 0.8 Pa.

[0092] Specifically, in step S33, the vacuum chamber 10 is filled with argon gas, and the pressure of the chamber 10 is controlled to be 20000Pa.

[0093] The method for preparing the zirconium fiber ceramic crucible described in this embodiment comprises the following steps:

[0094] (1) Weighing zirconia ceramic fiber and a dispersant, wherein the dispersant is polyacrylamide, and the weight ratio of the polyacrylamide is 0.4% of the zirconia ceramic fiber, and fully stirring and mixing the zirconia ceramic fiber and the polyacrylamide to form a mixed liquid; weighing water and a binder, wherein the binder is silica sol, and the silica sol has a silicon oxide content of 30%, and the weight ratio of water to silica sol is 6:1, and fully stirring and mixing the water and the silica sol to form a slurry; then adding the mixed liquid to the slurry, and fully stirring and mixing to obtain a slurry, wherein the slurry density is 280 g / 100 ml; and then using the slurry to prepare a zirconia ceramic fiber crucible.

[0095] (2) Weighing fused yttrium oxide powder and silica sol, wherein the weight ratio of the fused yttrium oxide powder to the silica sol is 5:1, stirring the fused yttrium oxide powder and the silica sol to fully mix them to prepare a highly inert coating material resistant to titanium liquid corrosion; uniformly coating the prepared highly inert coating material resistant to titanium liquid corrosion on the inner surface of the zirconia ceramic fiber crucible, and then drying to obtain a zirconium fiber ceramic crucible.

[0096] Example 2

[0097] In this embodiment, different from the embodiment 1,

[0098] Specifically, in step S1, the diameter of the titanium and titanium alloy ingot is 48.8 mm and the length is 212.4 mm.

[0099] Specifically, in step S1, the surface pickling treatment time is 10 minutes.

[0100] Specifically, in step S34, the power of the smelting power supply 2 is increased to 220kw.

[0101] Specifically, in step S35, the smelting power supply 2 is turned off, and the ceramic mold shell is left to stand in the furnace chamber for 3.5 minutes to cool. After the titanium and titanium alloy melt in the ceramic mold shell are completely solidified, the ceramic mold shell is taken out from the furnace chamber, and after the ceramic mold shell is cooled to 280°C, the ceramic mold shell is broken and the cast titanium alloy watch case casting is taken out.

[0102] Specifically, in step S33, the vacuum chamber 10 is filled with argon gas, and the pressure of the chamber 10 is controlled to be 30000Pa.

[0103] Example 3

[0104] In this embodiment, different from the embodiment 1,

[0105] Specifically, in step S34, the power of the smelting power supply 2 is increased to 200kw.

[0106] Example 4

[0107] In this embodiment, different from the embodiment 1,

[0108] Specifically, in step S34, the power of the smelting power supply 2 is increased to 250kw.

[0109] Example 5

[0110] In this embodiment, different from the embodiment 1,

[0111] Specifically, this embodiment provides a method for preparing a titanium watch case casting, and the material used in this embodiment is pure titanium. The melting time of titanium and titanium alloy ingots during casting in the preparation methods of titanium and titanium alloy watch case castings described in Examples 1 to 5 is monitored and counted, as shown in Table 1.

[0112] Table 1

[0113]

[0114] It can be seen from Table 1 that in the preparation method of titanium and titanium alloy watch case castings described in Examples 1 to 5, the power of the smelting power supply 2 is increased to 200-250 kW, which can achieve the melting of titanium and titanium alloy ingots within 1 minute, greatly improving the production efficiency of titanium and titanium alloy castings, and effectively ensuring the large-scale rapid production of titanium and titanium alloy castings.

[0115] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for preparing titanium and titanium alloy watch case castings, characterized in that: The preparation method comprises the following steps: S1. Preparation of titanium and titanium alloy ingots: processing titanium and titanium alloy ingots to obtain titanium and titanium alloy ingots; S2, shell preparation: prepare a wax mold and a mold frame (11), weld the wax mold assembly to the mold frame (11); then bond the mold frame (11) and the zircon fiber ceramic crucible together; prepare a shell surface layer and a shell back layer for the mold frame (11) and the zircon fiber ceramic crucible, the number of prepared layers is 5 and a half; then dewax treatment is performed, and finally roasting is performed to prepare a ceramic shell for casting; S3, casting and molding: placing a titanium or titanium alloy ingot in a zirconium fiber ceramic crucible, placing the ceramic shell containing the titanium or titanium alloy ingot in a vacuum induction rapid melting furnace for melting, increasing the power of the melting power source (2) to 215-250 kW, and rapidly melting the titanium or titanium alloy ingot within 1 minute to form a titanium or titanium alloy casting; then stopping the furnace for cooling to obtain a cast titanium or titanium alloy watch case casting; Step S3 includes the following steps: S31, loading the mold shell into the furnace: taking out the fired ceramic mold shell, placing the titanium and titanium alloy round ingots in the zirconium fiber ceramic crucible, placing the ceramic mold shell loaded with the titanium and titanium alloy round ingots in the cavity (10) of the vacuum induction rapid melting furnace, and sealing it; S32, evacuating: starting the vacuum pump device (1) of the sealed vacuum induction rapid melting furnace to evacuate the cavity (10); S33, argon backfilling: filling the vacuum chamber (10) with argon; S34, heating and melting: starting the melting power source (2), increasing the power of the melting power source (2) to 215-250 kW, and rapidly filling the molten titanium and titanium alloy into the ceramic mold shell under the action of gravity to form titanium and titanium alloy castings; S35, stopping the furnace for cooling: turning off the melting power supply (2), leaving the ceramic shell in the furnace cavity for 2 to 4 minutes to cool, and waiting for the titanium and titanium alloy melt in the ceramic shell to completely solidify, taking out the ceramic shell from the cavity (10), and waiting for the ceramic shell to cool to below 300° C., breaking the ceramic shell, and taking out the cast titanium alloy watch case casting; In step S2, the calcination temperature is 950°C and the holding time is 4h; In step S2, after preparing a wax mold and a mold frame (11) for forming a titanium alloy watch case, the prepared wax mold and mold frame (11) are placed in a constant temperature and humidity workshop for a period of ≥4 hours. After the size of the wax mold and the mold frame (11) shrinks and stabilizes, the wax mold assembly is welded to the mold frame (11); In step S32, the cavity (10) is evacuated to make the vacuum degree in the cavity (10) less than 0.9 Pa; In step S33, the vacuum chamber (10) is filled with argon gas, and the pressure of the chamber (10) is controlled to be 20000-30000 Pa; The wall thickness of the titanium and titanium alloy watch case casting is less than 1mm; In step S1, the diameter of the titanium and titanium alloy ingot is 48-50 mm and the length is 180-220 mm; The raw materials of the zirconium fiber ceramic crucible include zirconium oxide ceramic fiber, a dispersant and a binder, and the inner surface of the zirconium fiber ceramic crucible has a highly inert titanium liquid corrosion-resistant coating; The dispersant is polyacrylamide, and the weight of the polyacrylamide accounts for 0.4% of the zirconia ceramic fiber. The zirconia ceramic fiber and polyacrylamide are fully stirred and mixed into a mixed liquid; water and a binder are weighed, the binder is silica sol, the silicon oxide content in the silica sol is 30%, and the weight ratio of water to silica sol is 6:

1. Water and silica sol are fully stirred and mixed to form a slurry; then the mixed liquid is added to the slurry, and the slurry is fully stirred and mixed to obtain a slurry, and the slurry density is 280g / 100ml; and then the slurry is used to prepare a zirconium fiber ceramic crucible.

2. The method for preparing a titanium and titanium alloy watch case casting according to claim 1, characterized in that: Step S1 specifically includes: subjecting the titanium and titanium alloy ingots to sizing, surface lathing, surface polishing, surface pickling and water washing, and then drying to prepare titanium and titanium alloy round ingots.

3. The method for preparing a titanium and titanium alloy watch case casting according to claim 2, characterized in that: In step S1, an acid solution is used in the surface pickling treatment, wherein the acid solution includes water, nitric acid and hydrofluoric acid, the weight ratio of water, nitric acid and hydrofluoric acid is 8:3:2, and the surface pickling treatment time is 5 to 10 minutes.

4. A titanium and titanium alloy watch case casting, characterized in that: The titanium and titanium alloy watch case casting is prepared using the method for preparing the titanium and titanium alloy watch case casting described in any one of claims 1 to 3.