Silicon carbide / graphite composite material and preparation method thereof

By adopting a combined structure of intermediate coating and dense silicon carbide coating in silicon carbide/graphite composite materials, the thermal mismatch between the coating and the substrate and cracking of graphite materials is solved, and the stability and use of materials are significantly improved. life.

CN118515503BActive Publication Date: 2024-11-26ZHEJIANG LIUFANG CARBON TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410990154.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-26
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

The existing silicon carbide/graphite composite materials have accumulated stress between the coating and the substrate due to lattice mismatch under temperature changes, resulting in unstable coating and reduced lifetime, and graphite materials are prone to cracking, affecting service life.

Method used

Using an intermediate coating, including a first sub-layer close to the silicon carbide coating and a second sub-layer close to the graphite substrate, in which the silicon carbide is filled along the graphite pore wall to form a continuous wall layer, and in the second sub-layer, the silicon carbide is Discretely distributed particles are formed in the graphite pores, and an intermediate coating is formed by chemical vapor phase reaction to alleviate the thermal mismatch problem, and a dense silicon carbide coating is formed outside the surface of the intermediate coating to improve bond strength.

Benefits of technology

It improves the flexural strength and compressive strength of graphite materials, prevents cracking, enhances the bonding force between the coating and the graphite matrix, extends the service life of graphite materials, and improves the overall stability of composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118515503B_ABST
    Figure CN118515503B_ABST
Patent Text Reader

Abstract

The present invention discloses a silicon carbide / graphite composite material and a preparation method thereof, and relates to the field of graphite / coating composite materials. The silicon carbide / graphite composite material comprises a graphite substrate, an intermediate coating and a silicon carbide coating, wherein the intermediate coating is connected to the graphite substrate and the silicon carbide coating; the intermediate coating comprises a first sublayer close to the silicon carbide coating and a second sublayer close to the graphite substrate, wherein both the first sublayer and the second sublayer contain graphite and silicon carbide; in the first sublayer, part of the silicon carbide fills along the graphite pore wall and forms a continuous wall layer on the graphite pore wall, and part of the silicon carbide forms a continuous film layer along the graphite surface, wherein the wall layer is connected to the film layer; in the second sublayer, silicon carbide forms discretely distributed silicon carbide particles in the graphite pores. The intermediate coating can play a good transition role, which is conducive to alleviating the thermal mismatch problem between the graphite substrate and the coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of graphite / coating composite materials, and in particular to a silicon carbide / graphite composite material and a preparation method thereof. Background Art

[0002] Isostatic graphite materials play an important role in the semiconductor industry due to their excellent thermal conductivity and stability. They can not only be used as substrate materials, but also play a key role in electronics, optoelectronics, sensors and energy storage. However, if only pure graphite materials are used, there will be some problems: graphite easily reacts with oxygen to produce oxidation consumption; graphite is soft and easy to wear; graphite is affected by hydrogen, ammonia corrosive gases and residual metal organic matter at high temperatures, which may cause corrosion and / or powder shedding, thereby significantly reducing its service life and may also cause pollution to the product. In order to meet this challenge, coating technology has become the main solution, which can achieve the purpose of fixing surface powder, improving thermal conductivity and evenly distributing heat.

[0003] The most commonly used coating at present is silicon carbide coating. SiC coating products are widely used in the semiconductor industry, such as silicon single crystal growth, silicon epitaxy, silicon carbide epitaxy, MOCVD (metal organic chemical vapor deposition), etc. However, there is a mismatch between the lattice constant or thermal expansion coefficient of the SiC coating and the substrate material (such as graphite). Under temperature changes, stress accumulation between the coating and the substrate will occur, thereby affecting the stability of the coating. The coating will crack or peel off, resulting in coating instability and reduced life. During the use of graphite materials, problems such as graphite cracking may also occur, which seriously affects the service life of graphite materials.

[0004] Therefore, the current silicon carbide / graphite composite materials and preparation methods thereof still need to be improved. Summary of the invention

[0005] The present invention aims to alleviate or solve at least one of the above-mentioned problems to at least some extent.

[0006] In one aspect of the present invention, the present invention proposes a silicon carbide / graphite composite material. According to some embodiments of the present invention, the silicon carbide / graphite composite material includes a graphite substrate, an intermediate coating and a silicon carbide coating, wherein the intermediate coating is connected to the graphite substrate and the silicon carbide coating; the intermediate coating includes a first sublayer close to the silicon carbide coating and a second sublayer close to the graphite substrate, wherein the first sublayer and the second sublayer both contain graphite and silicon carbide; in the first sublayer, part of the silicon carbide fills along the graphite pore wall and forms a continuous wall layer on the graphite pore wall, and part of the silicon carbide forms a continuous film layer along the graphite surface, wherein the wall layer is connected to the film layer; in the second sublayer, silicon carbide forms discretely distributed silicon carbide particles in the graphite pore. The intermediate coating can play a good transition role, which is conducive to alleviating the thermal mismatch problem between the graphite substrate and the coating; the second sublayer can increase the flexural strength and compressive strength of the graphite, improve the overall strength of the graphite, prevent the graphite from cracking, and improve the bonding force between the entire intermediate coating and the graphite.

[0007] According to some embodiments of the present invention, in the first sublayer, the porosity of silicon carbide of the wall layer is less than 2%, the wall thickness of the wall layer is 0.2 μm-2 μm, the porosity of silicon carbide of the membrane layer is less than 2%, and the thickness of the membrane layer is 0.2 μm-10 μm.

[0008] According to some embodiments of the present invention, in the second sub-layer, the size of the silicon carbide particles is 10 nm-5 μm, and the size of the graphite pores is 1 μm-40 μm.

[0009] According to some embodiments of the present invention, the depth of the intermediate coating is greater than or equal to 100 μm, thereby improving the bonding strength between the coating and the graphite substrate, and the intermediate coating can provide better adhesion for the silicon carbide coating on the surface, thereby preventing the coating from cracking or falling off.

[0010] In another aspect of the present invention, the present invention provides a method for preparing the silicon carbide / graphite composite material mentioned above. According to some embodiments of the present invention, a method for preparing the aforementioned silicon carbide / graphite composite material comprises the following steps: step (1): placing a graphite substrate in a reaction chamber, introducing a first silicon source, argon and hydrogen into the reaction chamber at a first temperature and a first pressure to deposit an intermediate coating, the deposition time being 2h-10h, the flow rate of the first silicon source being 1.5slm-15slm, the first temperature being 1300°C-1700°C, and the first pressure being 6000Pa-70000Pa; step (2): adjusting the temperature and pressure in the reaction chamber to a second temperature and a second pressure, introducing a second silicon source, argon and hydrogen into the reaction chamber, the second silicon source containing carbon, or introducing a third silicon source, a carbon source, argon and hydrogen into the reaction chamber, the third carbon source not containing carbon, forming a silicon carbide coating on a side of the intermediate coating away from the graphite substrate, the second temperature being 1000°C-1400°C, and the second temperature being lower than the first temperature, and the second pressure being 100Pa-30000Pa. Through chemical vapor reaction, the first silicon source is infiltrated into the pores of graphite at high temperature to directly react with the graphite matrix to generate an intermediate coating, which includes two sublayers. The silicon carbide in the second sublayer is spherical particles. The second sublayer is used as a micro transition layer to increase the flexural strength and compressive strength of graphite, improve the overall strength of graphite, prevent graphite cracking, and improve the bonding force between the entire transition layer and graphite. The intermediate coating is mainly formed under the conditions of high deposition pressure and large gas flow in this scheme. In the first sublayer, part of the silicon carbide fills along the graphite pore wall and forms a continuous wall layer, and part of the silicon carbide forms a continuous film layer along the graphite surface. The wall layer is connected to the film layer. After the intermediate coating is formed, a dense silicon carbide coating is formed on the surface of the intermediate coating by chemical vapor deposition (CVD). The properties of the film layer are similar to those of the silicon carbide coating, so that the silicon carbide coating and the intermediate coating can be firmly bonded, thereby alleviating the thermal mismatch problem between the coating and the graphite matrix at least to a certain extent, and is conducive to improving the bonding strength between the coating and the graphite matrix.

[0011] According to some embodiments of the present invention, in step (1), the first silicon source includes at least one of silicon tetrachloride, chlorosilane, dichlorosilane, trichlorosilane and silane. The above materials can penetrate into the pores of graphite at high temperature, react with the graphite matrix to generate silicon carbide, and the graphite and silicon carbide form an intermediate coating.

[0012] According to some embodiments of the present invention, in step (1), the flow rate of argon is 1slm-50slm, and the flow rate of hydrogen is 1slm-200slm. The addition of argon is beneficial to improving the safety of the reaction; the flow rates of argon and hydrogen are within the above range, which is beneficial to the formation of the intermediate coating.

[0013] According to some embodiments of the present invention, in step (2), the second silicon source includes trichloromethylsilane, and the flow rate of the second silicon source is 0.5slm-100slm. Thus, the second silicon source can form a silicon carbide coating on the side of the intermediate coating away from the graphite substrate through a chemical vapor deposition reaction, and the bonding strength between the silicon carbide coating and the intermediate coating is relatively high, which is beneficial to further improve the stability of the silicon carbide / graphite composite material, thereby helping to extend the service life of the graphite material.

[0014] According to some embodiments of the present invention, in step (2), a second silicon source, argon and hydrogen are introduced into the reaction chamber, the flow rate of argon is 0.5slm-200slm, the flow rate of hydrogen is 0.5slm-200slm, and the ratio of the flow rate of hydrogen to the flow rate of the second silicon source is 1-50.

[0015] According to some embodiments of the present invention, in step (2), the third silicon source includes at least one of silane, monochlorosilane, dichlorosilane, trichlorosilane and silicon tetrachloride, the carbon source includes at least one of methane, propylene, ethylene and acetylene, the flow rate of the third silicon source is 0.5slm-100slm, and the flow rate of the carbon source is 0.5slm-100slm.

[0016] According to some embodiments of the present invention, in step (2), a third silicon source, a carbon source, argon and hydrogen are introduced into the reaction chamber, the flow rate of argon is 0.5slm-200slm, the flow rate of hydrogen is 0.5slm-200slm, and the ratio of the flow rate of hydrogen to the flow rate of the third silicon source is 1-50.

[0017] According to some embodiments of the present invention, in step (2), the deposition time of the silicon carbide coating is 1 hour to 20 hours, thereby forming a silicon carbide coating with a suitable thickness in a relatively short time, thereby further improving the stability of the silicon carbide / graphite composite material. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0019] Figure 1 A schematic structural diagram of a silicon carbide / graphite composite material according to an embodiment of the present invention is shown;

[0020] Figure 2 shows a cross-sectional scanning electron microscope photograph of the silicon carbide / graphite composite material in Example 3 of the present invention;

[0021] Figure 3shows a cross-sectional scanning electron microscope photograph of the intermediate coating and the silicon carbide coating in Example 4 of the present invention;

[0022] Figure 4 shows a cross-sectional scanning electron microscope photograph of the first sublayer in Example 4 of the present invention;

[0023] Figure 5 A locally enlarged scanning electron microscope photograph of the first sublayer in Example 4 of the present invention is shown;

[0024] Figure 6 A scanning electron microscope photograph of a cross section of the first sublayer and the second sublayer in Example 4 of the present invention is shown;

[0025] Figure 7 A locally enlarged scanning electron microscope photograph of the first sublayer in Example 4 of the present invention is shown;

[0026] Figure 8 A local magnified scanning electron microscope photograph of the second sublayer in Example 4 of the present invention is shown;

[0027] Fig. 9 shows the XRD spectrum of the intermediate coating in Example 4 of the present invention;

[0028] Fig.10 shows the XRD spectrum of the silicon carbide coating in Example 4 of the present invention;

[0029] Fig.11 shows a scanning electron microscope photograph of the sample in Comparative Example 1;

[0030] Fig.12 shows a scanning electron microscope photograph of the sample in Comparative Example 2;

[0031] Fig.13 shows a scanning electron microscope photograph of the sample in Comparative Example 3;

[0032] Fig.14 A scanning electron microscope photograph of the sample in Comparative Example 4 is shown.

[0033] Description of reference numerals:

[0034] 1: silicon carbide coating; 2: intermediate coating; 3: graphite substrate; 4: silicon carbide; 5: graphite; 6: cavity; 7: hole; 8: first sublayer; 9: second sublayer; 11: wall layer; 12: membrane layer; 13: graphite pores; 14: silicon carbide particles. DETAILED DESCRIPTION

[0035] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0036] In one aspect of the present invention, the present invention provides a silicon carbide / graphite composite material. According to some embodiments of the present invention, reference Figure 1 and Figure 2 The silicon carbide / graphite composite material may include a graphite substrate 3, an intermediate coating 2 and a silicon carbide coating 1, wherein the intermediate coating 2 is connected to the graphite substrate 3 and the silicon carbide coating 1.

[0037] refer to Figure 1 and Figure 2 The intermediate coating 2 may include a first sublayer 8 close to the silicon carbide coating 1 and a second sublayer 9 close to the graphite substrate 3. Both the first sublayer 8 and the second sublayer 9 contain graphite and silicon carbide. In the first sublayer 8, part of the silicon carbide fills along the graphite pore wall and forms a continuous wall layer 11 on the graphite pore wall, and part of the silicon carbide forms a continuous film layer 12 along the graphite surface, and the wall layer 11 is connected to the film layer 12. In the second sublayer 9, silicon carbide forms discretely distributed silicon carbide particles 14 in the graphite pore 13. The second sublayer, as a micro-transition layer, is a film layer with a low silicon carbide content in the intermediate coating. The thermal expansion coefficient and mechanical properties of the second sublayer are between the first sublayer and the graphite substrate, and can play a good transition role. The second sublayer can increase the flexural strength and compressive strength of the graphite substrate, improve the overall strength of the graphite material, and prevent graphite cracking. At the same time, it can also make the expansion coefficient of graphite slowly approach the thermal expansion coefficient of the silicon carbide coating on the surface, and improve the bonding strength between the entire intermediate coating and the graphite substrate. The first sublayer is close to the silicon carbide coating. Part of the silicon carbide fills along the graphite pore wall and forms a continuous wall layer on the graphite pore wall. Part of the silicon carbide forms a continuous film layer along the graphite surface. The first sublayer is like a "tree root in the soil" that firmly connects the graphite and the silicon carbide coating on the surface. The silicon carbide content of this layer is high, and the thermal expansion coefficient and mechanical properties are relatively close to the silicon carbide coating on the surface. The intermediate coating is used to transition between the graphite substrate and the silicon carbide coating, which can make the coating and graphite have a higher bonding strength. The thermal expansion coefficient and mechanical properties of the intermediate coating gradually change, which significantly improves the thermal mismatch problem between the graphite and the coating. The graphite material is not prone to cracking or shedding of the coating; and it can at least prevent graphite cracking to a certain extent, extending the service life of the graphite material.

[0038] According to some embodiments of the present invention, reference Figure 1 and Figure 2The component of the surface of the intermediate coating 2 in contact with the silicon carbide coating 1 is silicon carbide, that is, the surface of the intermediate coating 2 away from the graphite substrate 3 is a silicon carbide film, which can be firmly bonded to the subsequently formed silicon carbide coating, thereby improving the overall bonding strength between the coating and the graphite substrate.

[0039] According to some embodiments of the present invention, reference Figure 1 and Figure 2 In the first sublayer 8, the porosity of silicon carbide in the wall layer 11 is less than 2%, and the wall thickness of the wall layer 11 can be 0.2μm-2μm. For example, the porosity of silicon carbide in the wall layer 11 can be ≤1%, ≤1.3%, ≤1.5% or ≤1.9%, and the wall thickness of the wall layer 11 can be 0.2μm, 0.5μm, 0.6μm, 0.8μm, 1μm, 1.5μm, 2μm, etc. The porosity of silicon carbide in the membrane layer 12 is less than 2%, and the thickness of the membrane layer 12 can be 0.2μm-10μm. For example, the porosity of silicon carbide in the membrane layer 12 can be ≤1%, ≤1.3%, ≤1.5% or ≤1.9%, and the thickness of the membrane layer 12 can be 0.2μm, 0.5μm, 1μm, 3μm, 5μm, 8μm, 10μm, etc.

[0040] According to some embodiments of the present invention, reference Figure 1 and Figure 2 In the second sublayer 9, the size of the silicon carbide particles 14 may be 10 nm-5 μm, and the size of the graphite pores 13 may be 1 μm-40 μm. For example, in the second sublayer 9, the size of the silicon carbide particles 14 may be 10 nm, 50 nm, 100 nm, 1 μm, 3 μm, 5 μm, etc., and the size of the graphite pores 13 may be 1 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, etc.

[0041] According to some embodiments of the present invention, in the silicon carbide / graphite composite material, the depth of the intermediate coating 2 may be greater than or equal to 100 μm, for example, the depth of the intermediate coating 2 may be 100 μm-1000 μm, specifically, the depth of the intermediate coating may be 100 μm, 200 μm, 400 μm, 500 μm, 600 μm, 800 μm, 1000 μm, etc. The depth of the intermediate coating is greater than or equal to 100 μm, the intermediate coating may be firmly bonded to the graphite substrate, and may provide greater adhesion for the subsequently formed silicon carbide coating, which is beneficial to improving the bonding strength between the subsequently formed silicon carbide coating and the intermediate coating, thereby facilitating improving the overall stability of the graphite material.

[0042] According to some embodiments of the present invention, the depth of the intermediate coating may be greater than or equal to 200 μm, for example, the depth of the intermediate coating may be 200 μm-1000 μm.

[0043] In another aspect of the present invention, the present invention provides a method for preparing the aforementioned silicon carbide / graphite composite material. According to some embodiments of the present invention, the method for preparing the aforementioned silicon carbide / graphite composite material may include the following steps:

[0044] Step (1): placing a graphite substrate in a reaction chamber, introducing a first silicon source, argon and hydrogen into the reaction chamber at a first temperature and a first pressure to deposit an intermediate coating, the deposition time being 2h-10h, the flow rate of the first silicon source being 1.5slm-15slm, the first temperature being 1300°C-1700°C, and the first pressure being 6000Pa-70000Pa. At a higher deposition pressure and temperature, the flow rate of the silicon source is larger, and the silicon source can penetrate into the pores of the graphite and react directly with the graphite substrate to generate an intermediate coating. Reference Figure 1 and Figure 2 , along the direction close to the graphite substrate 3, the intermediate coating 2 may include a first sublayer 8 and a second sublayer 9 stacked in sequence, both of which contain graphite and silicon carbide. In the first sublayer 8, part of the silicon carbide fills along the graphite pore wall and forms a continuous wall layer 11 on the graphite pore wall, and part of the silicon carbide forms a continuous film layer 12 along the graphite surface, and the wall layer 11 is connected to the film layer 12; in the second sublayer 9, silicon carbide forms discretely distributed silicon carbide particles 14 in the graphite pore 13. A longer deposition time can form an intermediate coating with a suitable thickness, thereby improving the thermal mismatch problem between silicon carbide and the graphite substrate and improving the bonding strength between the coating and the graphite substrate.

[0045] Under the high pressure and high flow conditions of this scheme, an intermediate coating of the above structure is formed, which can provide an appropriate interface or serve as a transition material layer for the graphite substrate and the silicon carbide coating formed by subsequent deposition. In the vertical direction (thickness direction), the silicon carbide content, thermal expansion coefficient, and mechanical properties of the intermediate coating gradually change, which helps to smoothly transition the properties of the upper and lower materials, reduce the stress caused by the sudden change, and can effectively improve the bonding strength between the coating and the substrate, so that the coating is not easy to crack after high and low temperature thermal cycles. The intermediate coating can provide better adhesion for the silicon carbide coating formed subsequently, so that the coating adheres firmly to the surface of the substrate and prevents the coating from cracking or falling off. The intermediate coating can provide a smooth surface, which helps to form a more uniform interface between the SiC coating prepared by subsequent CVD and the graphite substrate, and helps to deposit a uniform SiC coating thereon to ensure the uniformity and consistency of the coating. The intermediate coating can also reduce the surface roughness of the coating formed subsequently, thereby adjusting the surface properties of the coating so that the graphite material can adapt to different application requirements.

[0046] According to some embodiments of the present invention, the deposition time of the intermediate coating can be 2h, 3h, 4h, 5h, 6h, 7h, 8h or 10h. The deposition time within the above range is conducive to the full reaction of the first silicon source and the graphite substrate. The first silicon source can penetrate into the graphite substrate to a certain depth to obtain an intermediate coating of appropriate thickness, which is beneficial to provide better adhesion for the subsequent silicon carbide coating on the surface.

[0047] According to some embodiments of the present invention, the first temperature may be 1300°C, 1400°C, 1500°C, 1600°C, or 1700°C.

[0048] According to some embodiments of the present invention, the first pressure may be 6000Pa, 10000Pa, 20000Pa, 30000Pa, 40000Pa, 50000Pa or 70000Pa.

[0049] According to some embodiments of the present invention, the flow rate of the first silicon source can be 1.5slm, 2slm (standard litre per minute), 2.5slm, 3slm, 3.5slm, 4slm, 4.5slm, 6slm, 8slm, 10slm, 12slm or 15slm. The flow rate of the first silicon source within the above range is conducive to the first silicon source entering the interior of the graphite and reacting with the graphite to form silicon carbide, and is conducive to improving the bonding strength between the silicon carbide coating formed by subsequent CVD and the intermediate coating.

[0050] According to some embodiments of the present invention, in step (1), the first silicon source may include at least one of silicon tetrachloride, chlorosilane (one hydrogen atom in silane is replaced by a chlorine atom), dichlorosilane, trichlorosilane and silane. Specifically, the first silicon source may be silicon tetrachloride (SiCl 4 ), chlorosilane, dichlorosilane, trichlorosilane (SiHCl 3 ) or silane, or a mixture of two or more of silicon tetrachloride, chlorosilane, dichlorosilane, trichlorosilane and silane. Thus, the first silicon source can enter the graphite matrix under appropriate reaction conditions and react with graphite to generate silicon carbide.

[0051] According to some embodiments of the present invention, in step (1), the flow rate of argon gas can be 1slm-50slm. For example, the flow rate of argon gas can be 1slm, 2slm, 2.5slm, 3slm, 3.5slm, 4slm, 4.5slm, 5slm, 7slm, 8slm, 10slm, 20slm, 30slm, 40slm or 50slm. Ar is an inert gas and does not participate in chemical reactions as a diluent gas. If hydrogen is directly used as a diluent gas for experiments, it will be dangerous if the sealing is not good and a small amount of oxygen enters the reaction chamber. The presence of Ar can reduce the risk of the reaction. The argon gas of the above flow rate can also adjust the reaction pressure in step (1) to promote the formation of the intermediate coating. Moreover, argon gas has an influence on the control mode of the reaction and the type and orientation of the crystal, and has an influence on the formation and growth of the crystal nucleus. Argon gas can appropriately inhibit the reaction rate and promote the growth of the grains.

[0052] According to some embodiments of the present invention, in step (1), the flow rate of argon gas may be 1slm-10slm.

[0053] According to some embodiments of the present invention, in step (1), the flow rate of hydrogen is 1slm-200slm. For example, the flow rate of hydrogen can be 1slm, 2slm, 2.5slm, 3slm, 3.5slm, 4slm, 4.5slm, 5slm, 8slm, 10slm, 50slm, 100slm, 150slm or 200slm. Hydrogen can be used as a carrier gas and a dilution gas to carry silicon source gas, and can also be used as one of the reaction gases to directly participate in the deposition reaction.

[0054] According to some embodiments of the present invention, in step (1), the flow rate of hydrogen is 1slm-10slm.

[0055] According to some embodiments of the present invention, before placing the graphite substrate in the reaction chamber, the graphite substrate may be polished, ultrasonically cleaned and dried, thereby removing powder attached to the surface of the graphite substrate and reducing the surface roughness of the graphite substrate.

[0056] According to some embodiments of the present invention, after the graphite substrate is placed in the reaction chamber, a vacuum treatment may be performed first (for example, the pressure of the reaction chamber may be reduced to about 10 Pa), and then heating may be performed to raise the temperature of the reaction chamber to a first temperature. Thus, by removing the air in the reaction chamber before heating, the adverse effects of the air on the formation of silicon carbide in the subsequent reaction process may be avoided.

[0057] Step (2): adjusting the temperature and pressure in the reaction chamber to a second temperature and a second pressure, introducing a second silicon source, argon and hydrogen into the reaction chamber, wherein the second silicon source contains carbon, or introducing a third silicon source, a carbon source, argon and hydrogen into the reaction chamber, wherein the third silicon source does not contain carbon, to form a silicon carbide coating on a side of the intermediate coating away from the graphite substrate, wherein the second temperature may be 1000° C.-1400° C., and the second temperature is lower than the first temperature, and the second pressure may be 100 Pa-30000 Pa. According to some embodiments of the present invention, the second temperature may be 1000°C, 1200°C, 1220°C, 1250°C, 1270°C, 1290°C, 1300°C, 1350°C or 1400°C, and the second pressure may be 100Pa, 500Pa, 1000Pa, 5000Pa, 10000Pa, 15000Pa, 20000Pa, 25000Pa or 30000Pa. The above temperature and pressure are conducive to the second silicon source or the third silicon source and the carbon source to form a silicon carbide coating on the side of the intermediate coating away from the graphite substrate through chemical vapor deposition, thereby improving the stability of the graphite material and extending the service life of the graphite material.

[0058] According to some embodiments of the present invention, the silicon carbide coating may be located on the surface of the intermediate coating away from the graphite substrate, the silicon carbide coating is firmly bonded to the intermediate coating, and the bonding strength between the entire coating and the graphite substrate is relatively high.

[0059] According to some embodiments of the present invention, in step (2), the second silicon source may include trichloromethylsilane (MTS), and MTS may form a silicon carbide coating by chemical vapor deposition at a certain temperature and pressure.

[0060] According to some embodiments of the present invention, in step (2), the flow rate of the second silicon source may be 0.5slm-100slm, for example, the flow rate of the second silicon source may be 0.5slm, 0.8slm, 1slm, 1.5slm, 2slm, 2.5slm, 3slm, 3.5slm, 4slm, 6slm, 10slm, 50slm or 100slm. The flow rate of the second silicon source within the above range is conducive to generating a silicon carbide coating of suitable thickness in a shorter time, saving preparation time, and being more suitable for industrial production.

[0061] According to some embodiments of the present invention, in step (2), the third silicon source may include at least one of silane, monochlorosilane, dichlorosilane, trichlorosilane and silicon tetrachloride, and the carbon source may include at least one of methane, propylene, ethylene and acetylene.

[0062] According to some embodiments of the present invention, in step (2), the flow rate of the third silicon source can be 0.5slm-100slm, for example, the flow rate of the third silicon source can be 0.5slm, 1slm, 5slm, 10slm, 30slm, 50slm or 100slm, thereby facilitating the formation of a silicon carbide coating on the side of the intermediate coating away from the graphite substrate through chemical vapor deposition.

[0063] According to some embodiments of the present invention, in step (2), the flow rate of the carbon source can be 0.5slm-100slm, for example, the flow rate of the carbon source can be 0.5slm, 1slm, 5slm, 10slm, 30slm, 50slm or 100slm, thereby facilitating the formation of a silicon carbide coating on the side of the intermediate coating away from the graphite substrate through chemical vapor deposition.

[0064] According to some embodiments of the present invention, in step (2), the flow rate of argon gas can be 0.5slm-200slm, for example, the flow rate of argon gas can be 0.5slm, 0.8slm, 1slm, 1.5slm, 10slm, 50slm, 100slm or 200slm. When the flow rate of argon gas is within the above range, on the one hand, the reaction pressure can be adjusted to promote the formation of silicon carbide coating, and on the other hand, it can be used as a diluent and protective gas to make the reaction safer. On the other hand, argon gas has an effect on the crystal type and orientation of the reaction product, and also on the formation and growth of the crystal nucleus. The above flow rate of argon gas can appropriately inhibit the reaction rate and promote grain growth. It should be noted that in step (2), in both cases of introducing the second silicon source or the third silicon source and the carbon source, the flow rate of argon gas can be adjusted within the range of 0.5slm-200slm.

[0065] According to some embodiments of the present invention, in step (2), the flow rate of hydrogen can be 0.5slm-200slm, for example, the flow rate of hydrogen can be 0.5slm, 1slm, 5slm, 8slm, 8.5slm, 9slm, 9.5slm, 10slm, 15slm, 40slm, 80slm, 120slm or 200slm. In this step, hydrogen can be used as a carrier gas and a diluent gas to carry the silicon source gas, and can also be used as one of the reaction gases to directly participate in the deposition reaction. It should be noted that in step (2), in both cases of introducing the second silicon source or the third silicon source and the carbon source, the flow rate of hydrogen can be adjusted within the range of 0.5slm-200slm.

[0066] According to some embodiments of the present invention, in step (2), the flow rate ratio of hydrogen gas to the flow rate of the second silicon source can be 1-50. For example, the flow rate ratio of hydrogen gas to the flow rate of the second silicon source can be 1, 5, 10, 20 or 50. The flow rate ratio of hydrogen gas to the second silicon source within the above range is conducive to the formation of the silicon carbide coating.

[0067] According to some embodiments of the present invention, in step (2), the ratio of the flow rate of hydrogen to the flow rate of the third silicon source can be 1-50. For example, the ratio of the flow rate of hydrogen to the flow rate of the third silicon source can be 1, 10, 30, 40 or 50.

[0068] According to some embodiments of the present invention, in step (2), the deposition time of the silicon carbide coating may be 1 hour to 20 hours, for example, the deposition time of the silicon carbide coating may be 1 hour, 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4.5 hours, 5 hours, 10 hours or 20 hours. When the deposition time is within the above range, a silicon carbide coating having a suitable thickness may be formed, thereby facilitating the improvement of the stability of the graphite material.

[0069] In general, in the present invention, the intermediate coating is first prepared by chemical vapor reaction. Under high reaction temperature, reaction pressure and large flow rate, the first silicon source penetrates into the interior of the graphite substrate and reacts with the graphite to form silicon carbide. The intermediate coating includes two sub-layers. The silicon carbide content, thermal expansion coefficient and mechanical properties of the intermediate coating gradually transition. The second sub-layer can improve the flexural strength and compressive strength of the graphite substrate, improve the overall strength of the graphite, and prevent the graphite from cracking. The thermal expansion coefficients of the two sub-layers gradually approach the silicon carbide coating on the surface, which can play a good transition role. The first sub-layer is close to the silicon carbide coating, and a continuous silicon carbide film layer is formed on the graphite pore wall. The film layer is like "tree roots in the soil". "The graphite is firmly connected to the silicon carbide coating on the surface; a long deposition time can obtain an intermediate coating of suitable thickness; then, a dense silicon carbide coating is formed on the side of the intermediate coating away from the graphite substrate by a chemical vapor deposition method, and the intermediate coating provides better adhesion for the silicon carbide coating, so that the silicon carbide coating and the intermediate coating are firmly combined, and the silicon carbide in the intermediate coating and the silicon carbide in the silicon carbide coating are both β-phase silicon carbide with good crystallinity. The graphite substrate and the intermediate coating are well combined, and the intermediate coating and the silicon carbide coating are closely combined without stratification and pores, so that the prepared silicon carbide / graphite composite material has a strong bonding force between the intermediate coating and the graphite substrate, and the overall stability is high. The preparation method proposed in the present invention can effectively reduce the thermal stress caused by the thermal expansion difference between the inside of the graphite substrate and the SiC coating formed by CVD, can make the SiC coating formed by CVD more difficult to peel off, improve the coating cracks, shedding, wafer contamination and other phenomena that occur during use, increase the number of times the graphite material is used, and reduce costs while improving product quality, thereby improving yield and quality benefits, and promoting the development of the semiconductor industry.

[0070] The present invention will be described below by specific examples, and it will be appreciated by those skilled in the art that the following specific examples are only for illustrative purposes, and do not limit the scope of the present invention in any way. In addition, in the following examples, unless otherwise specified, the materials and equipment used are all commercially available. If in the following examples, specific processing conditions and processing methods are not clearly described, then conditions and methods known in the art can be used to process.

[0071] Example 1

[0072] Step 1: Preparation of intermediate coating.

[0073] The graphite substrate is polished, ultrasonically cleaned, and dried to remove the powder attached to the surface and reduce the roughness.

[0074] The graphite substrate sample is placed in the deposition reaction chamber, and the entire deposition system is evacuated to about 10Pa.

[0075] Heat the deposition reaction chamber with the homemade tooling, wait until the temperature reaches 1450℃, adjust the pressure in the reaction chamber to 50000Pa, and introduce SiCl 4 , Ar and H 2 , where SiCl 4 The flow rate of Ar is 5slm, the flow rate of H 2 The flow rate is 5 slm, and the deposition time is 5 hours to form an intermediate coating. In Example 1, the depth of the intermediate coating is 200 μm.

[0076] Step 2: Prepare SiC coating.

[0077] After the preparation of the intermediate coating in the first step is completed, the temperature of the deposition reaction chamber is directly reduced to 1300°C, the pressure is adjusted to 15000Pa, and the raw materials MTS, Ar and H are introduced. 2 , where the flow rate of MTS is 2slm, the flow rate of Ar is 2slm, and the flow rate of H 2 The flow rate was 10 slm and the deposition time was 2 h to obtain a SiC coating with a thickness of about 100 µm.

[0078] Example 2

[0079] Step 1: Preparation of intermediate coating.

[0080] The graphite substrate is ultrasonically cleaned and dried to remove the powder attached to the surface and reduce the roughness.

[0081] The graphite substrate sample is placed in the deposition reaction chamber, and the entire deposition system is evacuated to about 10Pa.

[0082] Heat the deposition reaction chamber until the temperature reaches 1650°C, adjust the pressure in the reaction chamber to 15000Pa, and introduce silane, Ar and H 2 , where the flow rate of silane is 5slm, the flow rate of Ar is 2slm, and the flow rate of H 2 The flow rate is 5 slm, and the deposition time is 3 hours to form an intermediate coating. In Example 2, the depth of the intermediate coating is 400 μm.

[0083] Step 2: Prepare SiC coating.

[0084] After the preparation of the intermediate coating in the first step is completed, the temperature of the deposition reaction chamber is directly reduced to 1200°C, the pressure is adjusted to 20000Pa, and the raw materials MTS, Ar and H are introduced. 2 , the flow rate of MTS is 0.5slm, the flow rate of Ar is 1slm, and the flow rate of H 2 The flow rate was 10 slm and the deposition time was 5 h to obtain a SiC coating with a thickness of about 100 µm.

[0085] Example 3

[0086] Step 1: Preparation of intermediate coating.

[0087] The graphite substrate is ultrasonically cleaned and dried to remove the powder attached to the surface and reduce the roughness.

[0088] The graphite substrate sample is placed in the deposition reaction chamber, and the entire deposition system is evacuated to about 10Pa.

[0089] The deposition reaction chamber with the self-made tooling was heated and the temperature reached 1550°C. The pressure in the reaction chamber was adjusted to 40000Pa and SiCl 4 , Ar and H 2 , where SiCl 4 The flow rate of Ar is 5slm, the flow rate of H 2 The flow rate is 50 slm and the deposition time is 4 hours to form an intermediate coating. In Example 3, the depth of the intermediate coating is 600 μm.

[0090] Step 2: Prepare SiC coating.

[0091] After the preparation of the intermediate coating in the first step is completed, the temperature of the deposition reaction chamber is directly reduced to 1250°C, the pressure is adjusted to 10000Pa, and the raw material SiCl is introduced. 4 , CH 4 , Ar and H 2 , where SiCl 4 The flow rate is 4slm, CH 4 The flow rate of Ar is 0.5slm, the flow rate of H 2The flow rate was 8 slm and the deposition time was 2 h to obtain a SiC coating with a thickness of about 100 µm.

[0092] The cross-sectional SEM photograph of the silicon carbide / graphite composite material prepared in Example 3 is as follows: Figure 2 As shown, it can be seen that the intermediate coating 2 is located on one side of the graphite substrate 3, and the silicon carbide coating 1 is located on the side of the intermediate coating 2 away from the graphite substrate 3. Along the direction away from the graphite substrate 3, the depth of the intermediate coating 2 is greater than 500 μm; the intermediate coating 2 includes a first sublayer 8 and a second sublayer 9.

[0093] Example 4

[0094] Step 1: Preparation of intermediate coating.

[0095] The graphite substrate is ultrasonically cleaned and dried to remove the powder attached to the surface and reduce the roughness.

[0096] The graphite substrate sample is placed in the deposition reaction chamber, and the entire deposition system is evacuated to about 10Pa.

[0097] Heat the deposition reaction chamber with the homemade tooling, wait until the temperature reaches 1600℃, adjust the pressure in the reaction chamber to 30000Pa, and introduce SiCl 4 , Ar and H 2 , where SiCl 4 The flow rate of Ar is 5slm, the flow rate of H 2 The flow rate is 45 slm and the deposition time is 4 hours to form an intermediate coating. In Example 4, the depth of the intermediate coating is 1000 μm.

[0098] Step 2: Prepare SiC coating.

[0099] After the preparation of the intermediate coating in the first step is completed, the temperature of the deposition reaction chamber is directly reduced to 1300°C, the pressure is adjusted to 15000Pa, and the raw materials MTS, Ar and H are introduced. 2 , where the flow rate of MTS is 4slm, the flow rate of Ar is 0.5slm, and the flow rate of H 2 The flow rate was 8 slm and the deposition time was 2 h to obtain a SiC coating with a thickness of about 100 µm.

[0100] Figure 3 The connection between the intermediate coating 2 and the silicon carbide coating 1 of the silicon carbide / graphite composite material in Example 4 is shown. Figure 3 It can be seen that the intermediate coating 2 and the silicon carbide coating 1 are tightly combined without delamination or pores.

[0101] Figure 4The cross-section of the first sublayer of the silicon carbide / graphite composite material in Example 4 is shown. Part of the silicon carbide 4 in the first sublayer exists inside the graphite material. The silicon infiltrated by the gas phase reacts with the carbon in the pore walls inside the graphite and is firmly combined with the graphite matrix to form a wall layer 11. In addition, part of the silicon carbide reacts with the carbon on the surface of the graphite matrix to generate a continuous film layer 12. The wall layer 11 is connected to the film layer 12, further strengthening the combination of the intermediate coating and the graphite matrix.

[0102] Figure 5 A local enlarged SEM photograph of the first sublayer of the intermediate coating in Example 4 is shown. The intermediate coating contains graphite 5 and silicon carbide 4. The silicon carbide forms a wall layer 11 with a certain thickness on the graphite pore wall.

[0103] Figure 6 The cross-sectional SEM photograph of the first sublayer 8 and the second sublayer 9 in Example 4 is shown. Figure 6 It can be seen that the content of silicon carbide in the first sub-layer 8 is higher than the content of silicon carbide in the second sub-layer 9 .

[0104] Figure 7 A local enlarged SEM photograph of the first sublayer in Example 4 is shown. Figure 7 It can be seen that the silicon carbide in the first sublayer forms a wall layer of a certain thickness on the graphite pore wall.

[0105] Figure 8 A local enlarged SEM photo of the second sublayer in Example 4 is shown. Figure 8 It can be seen that the silicon carbide in the second sublayer forms spherical particles in the graphite pores, and the spherical particles are discretely distributed in the graphite pores.

[0106] Fig. 9 The XRD spectrum of the intermediate coating of Example 4 is shown. The black curve is the XRD spectrum obtained by the test. It can be seen that the intermediate coating contains 2H phase graphite and β phase silicon carbide. The silicon carbide has good crystallinity. It is calculated by software that the SiC content in the intermediate coating is 14.6%, and the graphite content is 85.4%.

[0107] Fig.10 The XRD spectrum of the silicon carbide coating of Example 4 is shown, and it can be seen that the coating is β-phase SiC with d(111) plane as the priority, and no other impurities. Fig. 9 and Fig.10 It can be seen that the silicon carbide in the intermediate coating layer is consistent with the silicon carbide in the silicon carbide coating layer, and both are β-phase silicon carbide with good crystallinity.

[0108] Example 5

[0109] The difference from Example 1 is that in the first step, the pressure in the reaction chamber is 6000 Pa. The remaining parameters and steps are the same as those in Example 1.

[0110] Example 6

[0111] Different from Example 2, in the first step, when the temperature reaches 1650°C, the pressure in the reaction chamber is adjusted to 70000Pa, and trichlorosilane, Ar and H are introduced. 2 , where the flow rate of trichlorosilane is 10slm, the flow rate of Ar is 5slm, and the flow rate of H 2 The flow rate is 100 slm. In Example 6, the depth of the intermediate coating is 800 μm. The remaining parameters and steps are the same as those in Example 2.

[0112] Example 7

[0113] The difference from Example 2 is that in the first step, the flow rate of silane is 1.5 slm. The remaining parameters and steps are the same as those in Example 2.

[0114] Example 8

[0115] Different from Example 4, in the first step, SiCl 4 The flow rate of Ar is 20slm, the flow rate of H 2 The flow rate is 200 slm and the deposition time is 2 hours. In Example 8, the depth of the intermediate coating is 700 μm. The remaining parameters and steps are the same as those in Example 4.

[0116] Example 9

[0117] The difference from Example 2 is that in the first step, the silicon source is monochlorosilane. The remaining parameters and steps are the same as those in Example 2.

[0118] Example 10

[0119] The difference from Example 3 is that in the first step, the silicon source is dichlorosilane, the flow rate of dichlorosilane is 4 slm, and the deposition time is 5 hours. In Example 10, the depth of the intermediate coating is 500 μm. The remaining parameters and steps are the same as those in Example 3.

[0120] Embodiment 11

[0121] The difference from Example 4 is that in the first step, the silicon source is trichlorosilane. The remaining parameters and steps are the same as those of Example 4.

[0122] Example 12

[0123] The difference from Example 4 is that in the first step, the temperature of the reaction chamber is 1300° C. and the deposition time is 8 hours. In Example 12, the depth of the intermediate coating is 300 μm. The remaining parameters and steps are the same as those of Example 4.

[0124] Comparative Example 1

[0125] The graphite substrate is ultrasonically cleaned and dried to remove the powder attached to the surface and reduce the roughness.

[0126] The graphite substrate sample is placed in the deposition reaction chamber, and the entire deposition system is evacuated to about 10Pa.

[0127] Heat the deposition reaction chamber until the temperature reaches 1650°C, adjust the pressure in the reaction chamber to 100000Pa, and introduce SiCl 4 , Ar and H 2 , where SiCl 4 The flow rate of Ar is 2slm, the flow rate of H 2 The flow rate was 5 slm and the deposition time was 3 h.

[0128] Different from Example 2, in Comparative Example 1, when SiCl 4 The pressure during chemical vapor infiltration reaction deposition coating is 100000Pa, SiCl 4 The flow rate is 60slm. The cross-sectional SEM photo of the sample prepared in Comparative Example 1 is as follows Fig.11 As shown, the pressure is too high, SiCl 4 The flow rate is too large, and it is difficult for the precursor to enter the interior of the graphite to react with it. It is easy to react on the surface to form a layer of silicon carbide 4 powder, and cause the surface of the graphite 5 to be stratified to form a cavity 6. The layer of silicon carbide 4 powder formed on the surface and the existence of the cavity 6 are not conducive to the combination with the silicon carbide coating formed by subsequent CVD, and the coating is easy to peel off or even fall off in the cavity.

[0129] Comparative Example 2

[0130] The graphite substrate is ultrasonically cleaned and dried to remove the powder attached to the surface and reduce the roughness.

[0131] The graphite substrate sample is placed in the deposition reaction chamber, and the entire deposition system is evacuated to about 10Pa.

[0132] The deposition reaction chamber with the self-made tooling was heated and the temperature reached 1550°C. The pressure in the reaction chamber was adjusted to 100000Pa and SiCl 4 , Ar and H 2 , where SiCl 4 The flow rate of Ar is 5slm, the flow rate of H 2 The flow rate is 5slm and the deposition time is 4h.

[0133] Different from Example 3, in Comparative Example 2, when SiCl 4The pressure during chemical vapor infiltration reaction deposition coating is 100000Pa, SiCl 4 The flow rate is 0.5slm. The cross-sectional SEM photo of the sample prepared in Comparative Example 2 is as follows Fig.12 As shown, the pressure is too high, SiCl 4 The flow rate is too small, and the precursor tends to react slowly with the graphite on the surface to form a loose coating on the surface of the graphite substrate. The loose coating of silicon carbide 4 has many holes 7 and no intermediate coating is formed.

[0134] Comparative Example 3

[0135] The graphite substrate is polished, ultrasonically cleaned, and dried to remove the powder attached to the surface and reduce the roughness.

[0136] The graphite substrate sample is placed in the deposition reaction chamber, and the entire deposition system is evacuated to about 10Pa.

[0137] Heat the deposition reaction chamber with the homemade tooling, wait until the temperature reaches 1450℃, adjust the pressure in the reaction chamber to 200Pa, and introduce SiCl 4 , Ar and H 2 , where SiCl 4 The flow rate of Ar is 5slm, the flow rate of H 2 The flow rate is 5slm and the deposition time is 5h.

[0138] Different from Example 1, in Comparative Example 3, when SiCl 4 The pressure during chemical vapor infiltration reaction deposition coating is 200Pa, SiCl 4 The flow rate is 1slm. The cross-sectional SEM photo of the sample prepared in Comparative Example 3 is as follows Fig.13 As shown, the pressure is too small, SiCl 4 The flow rate is too small, and the concentration of the precursor in the reaction chamber is too low, so it is difficult to form a relatively deep intermediate coating with a relatively high SiC content in a short time. According to the reaction conditions in Comparative Example 3, it may take thirty to forty hours or even longer to form an intermediate coating with a depth that meets the requirements, which is not suitable for industrial production.

[0139] Comparative Example 4

[0140] The graphite substrate is polished, ultrasonically cleaned, and dried to remove the powder attached to the surface and reduce the roughness.

[0141] The graphite substrate sample is placed in the deposition reaction chamber, and the entire deposition system is evacuated to about 10Pa.

[0142] Heat the deposition reaction chamber with the homemade tooling, heat the temperature of the deposition reaction chamber to 1300°C, adjust the pressure to 15000Pa, and introduce raw materials MTS, Ar and H 2 , where the flow rate of MTS is 2slm, the flow rate of Ar is 2slm, and the flow rate of H 2 The flow rate was 10 slm and the deposition time was 2 h to obtain a SiC coating with a thickness of about 100 µm.

[0143] The cross-sectional SEM photograph of the sample prepared in Comparative Example 4 is as follows: Fig.14 As shown, the silicon carbide coating 1 is directly formed on the surface of the graphite substrate 3 , and the components in the silicon carbide coating 1 do not penetrate into the graphite substrate 3 .

[0144] The scratch tester Rtec SMT5000 is used to test the bonding strength. The scratch tip automatically scratches the coating under a closed-loop loading force. Under a certain critical load, the coating will rupture and fail to test the bonding strength between the coating and the graphite substrate. The specific test conditions are shown in Table 1 below.

[0145] Table 1

[0146]

[0147] Three positions were taken for testing of each sample. The test data of the binding strength of the samples in Example 1 are recorded in Table 2, the test data of the binding strength of the samples in Example 4, Example 6, Example 8, Example 10 and Example 12 are recorded in Table 3, and the test data of the binding strength of the samples in Comparative Example 4 are recorded in Table 4.

[0148] Table 2

[0149]

[0150] In the early stage of scratching, the coating of the sample of Example 1 did not peel off. As shown in Table 2, when the loading force reached LC1, failure began, that is, peeling just occurred; when the loading force reached LC2, the coating peeled off over a large area, and the coating and the graphite substrate were delaminated.

[0151] Table 3

[0152]

[0153] The samples of Examples 4, 6, 8, 10 and 12 also had no peeling of the coating at the early stage of the scratch. As shown in Table 3, failure began to occur when the loading force reached LC1, i.e., peeling just occurred; when the loading force reached LC2, the coating peeled off over a large area, and the coating and the graphite substrate were delaminated.

[0154] It can be seen from the scratch test results of Examples 1 and 4 that when the depth of the intermediate coating increases from 200µm to 1000µm, the loading force at which the coating begins to fail and peels off increases from an average value of 12.62N to 28.76N, and the loading force at which large-area peeling occurs increases from an average value of 22.50N to 39.02N. It can be judged that, compared with Example 1, increasing the depth of the intermediate coating in Example 4 to 1000µm can significantly improve the bonding strength between the coating and the graphite substrate.

[0155] Table 4

[0156]

[0157] From the scratch test results in Table 4, it can be calculated that the average loading force at which the coating of the sample in Comparative Example 4 begins to fail and just begins to peel off is 10.06N, and the average loading force at which large-scale peeling occurs is 20.15N.

[0158] In addition, the loading force at which the coatings of the samples of Examples 2, 3, 5, 7, 9, and 11 just begin to peel off and the loading force at which large-scale peeling occurs are all higher than the test value of the sample in Comparative Example 4.

[0159] By comparison, it can be seen that compared with the direct use of the CVD method to form a silicon carbide coating on a graphite substrate in Comparative Example 4, the intermediate coating is first formed and then the silicon carbide coating is formed in the present invention, which can significantly improve the bonding strength between the coating and the graphite substrate.

[0160] In the description of the present invention, the orientation or position relationship indicated by the terms "upper" and "lower" etc. is based on the orientation or position relationship shown in the drawings and is only for the convenience of describing the present invention rather than requiring the present invention to be constructed and operated in a specific orientation. Therefore, it should not be understood as a limitation on the present invention.

[0161] In the description of this specification, the description with reference to the terms "one embodiment", "another embodiment", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment are included in at least one embodiment of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art can combine and combine the different embodiments or examples described in this specification and the features of different embodiments or examples, unless they are contradictory. In addition, it should be noted that in this specification, the terms "first", "second" and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated.

[0162] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a silicon carbide / graphite composite material, characterized in that: The following steps are involved: Step (1): placing a graphite substrate in a reaction chamber, introducing a first silicon source, argon and hydrogen into the reaction chamber at a first temperature and a first pressure to deposit an intermediate coating, The deposition time is 2 hours to 10 hours, the flow rate of the first silicon source is 1.5 slm to 15 slm, the first temperature is 1300° C. to 1700° C., and the first pressure is 6000 Pa to 70000 Pa; Step (2): adjusting the temperature and pressure in the reaction chamber to a second temperature and a second pressure, introducing a second silicon source, argon and hydrogen into the reaction chamber, wherein the second silicon source contains carbon, or introducing a third silicon source, a carbon source, argon and hydrogen into the reaction chamber, wherein the third silicon source does not contain carbon, forming a silicon carbide coating on the side of the intermediate coating away from the graphite substrate, wherein the second temperature is 1000° C. to 1400° C., and the second temperature is lower than the first temperature, and the second pressure is 100 Pa to 30000 Pa. In step (1), the first silicon source includes at least one of silicon tetrachloride, chlorosilane, dichlorosilane, trichlorosilane and silane, The silicon carbide / graphite composite material comprises a graphite substrate, an intermediate coating and a silicon carbide coating, wherein the intermediate coating is connected to the graphite substrate and the silicon carbide coating; The intermediate coating comprises a first sublayer close to the silicon carbide coating and a second sublayer close to the graphite substrate, wherein the first sublayer and the second sublayer both contain graphite and silicon carbide; In the first sublayer, part of the silicon carbide fills along the graphite pore wall and forms a continuous wall layer on the graphite pore wall, and part of the silicon carbide forms a continuous film layer along the graphite surface, and the wall layer is connected to the film layer; In the second sub-layer, silicon carbide forms discretely distributed silicon carbide particles in the graphite pores.

2. The method according to claim 1, characterized in that In the first sublayer, the porosity of the silicon carbide in the wall layer is less than 2%, and the wall thickness of the wall layer is 0.2 μm-2 μm. The porosity of the silicon carbide in the membrane layer is less than 2%, and the thickness of the membrane layer is 0.2 μm-10 μm.

3. The method according to claim 1, characterized in that In the second sub-layer, the size of the silicon carbide particles is 10 nm-5 μm, and the size of the graphite pores is 1 μm-40 μm.

4. The method according to claim 1, wherein The depth of the intermediate coating is greater than or equal to 100 μm.

5. The method according to claim 1, wherein In step (1), the flow rate of argon gas is 1slm-50slm, and the flow rate of hydrogen gas is 1slm-200slm.

6. The method according to claim 1, wherein In step (2), the second silicon source includes trichloromethylsilane, and the flow rate of the second silicon source is 0.5 slm-100 slm.

7. The method according to claim 6, characterized in that In step (2), the flow rate of argon is 0.5 slm-200 slm, the flow rate of hydrogen is 0.5 slm-200 slm, and the ratio of the flow rate of hydrogen to the flow rate of the second silicon source is 1-50.

8. The method according to claim 1, characterized in that In step (2), the third silicon source includes at least one of silane, monochlorosilane, dichlorosilane, trichlorosilane and silicon tetrachloride, the carbon source includes at least one of methane, propylene, ethylene and acetylene, the flow rate of the third silicon source is 0.5slm-100slm, and the flow rate of the carbon source is 0.5slm-100slm.

9. The method according to claim 8, characterized in that In step (2), the flow rate of argon is 0.5 slm-200 slm, the flow rate of hydrogen is 0.5 slm-200 slm, and the ratio of the flow rate of hydrogen to the flow rate of the third silicon source is 1-50.

10. The method according to any one of claims 1 to 9, characterized in that In step (2), the deposition time of the silicon carbide coating is 1 hour to 20 hours.