A mildew-proof and anti-slip TPE material and its preparation method and application in the preparation of toothbrush handles
Patent Information
- Application Number
- CN202411002437.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-25
AI Technical Summary
SEBS materials have insufficient antibacterial and mildew resistance and cannot be applied to materials that require antibacterial and mildew resistance, and their mechanical properties and wear resistance are also weak.
Elosite nanotube-based composite material reacts with polydopamine-modified bimetallic composite nanoparticles to form an organic-inorganic hybrid composite material, and graft polyethyleneimine and octadecamine on its surface, and add compound essential oil and nanometers Silica, which improves the antibacterial and mildew-proof properties of the material through specific process treatments.
It significantly improves the mechanical properties, wear resistance, anti-slip properties and long-lasting anti-bacterial and mildew resistance of TPE materials, ensures that the material has good bonding in the wet and dry interfaces, and enhances compatibility and dispersion in the SEBS matrix. sex.
Smart Images

Figure CN118515947B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, in particular to a mildew-proof and anti-slip TPE material and a preparation method thereof and application thereof in the preparation of toothbrush handles. Background Art
[0002] Thermoplastic elastomer (TPES) has attracted widespread attention due to its unique advantages. It has both the excellent processability of thermoplastics and the rubber properties. As one of the typical TPES polymers, styrene-ethylene-butylene-styrene block copolymer (SEBS) is known for its excellent anti-aging properties. However, its relatively weak mechanical strength and limited wear resistance limit its use. In order to change the mechanical properties of SEBS materials, Chinese patent application CN107880471A provides a high-tensile performance SEBS modified material and a preparation method thereof. The components of the SEBS modified material are calculated by weight as follows: 100 parts of SEBS, 50-100 parts of cyclohexane oil, 30 parts of polypropylene, 20-25 parts of polybutylene terephthalate, 10 parts of ethylene-butyl acrylate-glycidyl methacrylate copolymer, 30-40 parts of grafted blends, and 0.1-0.5 parts of antioxidants. The mechanical properties (tensile strength, elongation at break, hardness, etc.) of the high-tensile performance SEBS modified material have been greatly improved, but its antibacterial and mildew-proof properties need to be improved, and it cannot be applied to materials that require antibacterial and mildew-proof properties. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a method for preparing a mildew-proof and anti-slip TPE material, comprising the following steps:
[0004] Step (1), etching, amino modification, and carboxyl modification are performed on the halloysite nanotubes in sequence to obtain carboxylated halloysite nanotubes;
[0005] Step (2), loading the compound essential oil into the carboxylated halloysite nanotubes to obtain loaded modified halloysite nanotubes;
[0006] Step (3), first modifying the loaded modified halloysite nanotubes with chitosan, and then treating them with 2-(2-ethylene oxide)acetic acid to obtain a halloysite nanotube-based composite material; preparing bimetallic composite nanoparticles with copper nitrate trihydrate and tetrabutyl titanate as raw materials, and then modifying them with polydopamine to obtain polydopamine-modified bimetallic composite nanoparticles;
[0007] Step (4), reacting the halloysite nanotube-based composite material with polydopamine-modified bimetallic composite nanoparticles to obtain an organic-inorganic hybrid composite material, and grafting polyethyleneimine and octadecylamine on the surface of the organic-inorganic hybrid composite material to obtain a modified antibacterial and antifungal additive;
[0008] Step (5), mixing the modified SEBS, polypropylene and white oil, and then adding the modified antibacterial and mildew-proof additive, nano-silicon dioxide and antioxidant 1010 to obtain a mixture; melt-extrude the mixture, granulate, and cool to obtain a mildew-proof and anti-slip TPE material.
[0009] Preferably, in the step (1), the preparation method of the carboxylated halloysite nanotubes is as follows: at 40-60°C, the halloysite nanotubes are dispersed in a 5 mol / L sulfuric acid aqueous solution for etching for 12-16 hours, washed with deionized water and dried to obtain pretreated halloysite nanotubes; wherein the amount ratio of the halloysite nanotubes to the sulfuric acid aqueous solution is (5-10) g: (30-50) mL; the pretreated halloysite nanotubes are dispersed in toluene, ultrasonically treated for 100-150 min, and then 3-aminopropyltriethoxysilane is added, refluxed at 110-130°C for 12-16 hours, centrifuged, washed, and dried to obtain amino-treated halloysite nanotubes; wherein the mass ratio of the pretreated halloysite nanotubes, toluene, and 3-aminopropyltriethoxysilane is (3-6): ( 100-200): (7.5-18.9); at room temperature, suspending the aminated halloysite nanotubes in N,N-dimethylformamide, adding succinic anhydride, stirring the reaction for 20-28 hours, centrifuging, washing, and drying to obtain carboxylated halloysite nanotubes; wherein the mass ratio of the aminated halloysite nanotubes, N,N-dimethylformamide, and succinic anhydride is (3-6): (300-500): (40-70); in the above process, etching the halloysite nanotubes with sulfuric acid increases the specific surface area and pore volume of the halloysite nanotubes, thereby increasing the loading amount of the compound essential oil; introducing amino groups on the surface of the halloysite nanotubes by reacting 3-aminopropyltriethoxysilane with hydroxyl groups on the surface of the halloysite nanotubes, and introducing carboxyl groups on the surface of the halloysite nanotubes by reacting the amino groups with succinic anhydride.
[0010] Preferably, in step (2), the compound essential oil loading method is as follows: carboxylated halloysite nanotubes, compound essential oil and water are mixed in a mass ratio of 1: (2-3): (50-80), stirred for 20-30 minutes, then ultrasonically treated for 20-30 minutes, vacuum loaded at 0.01-0.012 atm for 30-40 minutes, restored to atmospheric pressure, repeated the vacuum loading 2-3 times, centrifuged, washed and dried; wherein the compound essential oil is composed of cinnamon essential oil and Litsea cubeba The essential oils are mixed in a mass ratio of (50-75): (25-50); in the above process, the compound essential oil is loaded in the carboxylated halloysite nanotubes by vacuum loading. The compound essential oil is obtained by mixing cinnamon essential oil and litsea cubeba essential oil. The main components of the compound essential oil are trans-cinnamaldehyde, citral a and citral b. Cinnamaldehyde and citral have antifungal and antibacterial effects on molds and bacteria. Due to the synergistic inhibitory effect, the combined use of cinnamon essential oil and litsea cubeba essential oil shows better effect than single use.
[0011] Preferably, in the step (3), the preparation method of the halloysite nanotube-based composite material is as follows: a chitosan acetic acid dispersion having a concentration of 0.8-1.2wt% and an essential oil-loaded halloysite nanotube aqueous dispersion having a concentration of 1-1.5wt% are mixed in equal volumes, stirred at room temperature for 20-30h, centrifuged, washed, and dried to obtain chitosan grafted loaded modified halloysite nanotubes; the chitosan grafted loaded modified halloysite nanotubes are dispersed in N,N-dimethylformamide, stirred for 20-40min, 2-(oxirane-2-yl)acetic acid is added, stirred at 70-90°C for 20-30h, centrifuged, and the precipitate obtained by centrifugation is purified by ethyl acetate. After washing with alcohol, water and acetone, the composite material is dried to obtain a halloysite nanotube-based composite material, wherein the mass ratio of chitosan graft-loaded modified halloysite nanotubes, N,N-dimethylformamide and 2-(2-oxirane-1-yl)acetic acid is (4-6): (150-300): (5-8). In the above process, chitosan and essential oil-loaded halloysite nanotubes are combined through electrostatic interaction between amino groups and carboxyl groups and hydrogen bonds to graft the chitosan cross-linked network structure onto the surface of the essential oil-loaded halloysite nanotubes. Furthermore, the amino groups in the chitosan react with the epoxy groups in the 2-(2-oxirane-1-yl)acetic acid to introduce carboxyl groups into the chitosan network structure.
[0012] Preferably, in step (3), the preparation method of the polydopamine modified bimetallic composite nanoparticles is as follows: copper nitrate trihydrate, tetrabutyl titanate, and ethanol are mixed in a mass ratio of 1: (0.5-1.2): (5-10), stirred for 10-30 minutes, stirred and reacted at 160-180°C for 7-9 hours, filtered, washed, and dried after the reaction to obtain bimetallic composite nanoparticles; ethanol, deionized water, 28wt% ammonia solution, and bimetallic composite nanoparticles are mixed, stirred at room temperature for 20-40 minutes, and then a 0.05g / mL dopamine hydrochloride aqueous solution is added, stirred and reacted for 6-8 hours, filtered, washed, and dried after the reaction to obtain polydopamine modified Bimetallic composite nanoparticles with a cuprous oxide heterostructure loaded with titanium dioxide are prepared by a one-pot solvothermal method using ethanol as a solvent and a reducing agent and copper nitrate trihydrate and tetrabutyl titanate as raw materials, wherein the bimetallic composite nanoparticles have an average particle size of about 20 nm, and then are modified by polydopamine to deposit mesoporous polydopamine (mesopore size is 4-40 nm) on the bimetallic composite nanoparticles.
[0013] Preferably, in the step (4), the preparation method of the modified antibacterial and mildew-proof additive is as follows: the halloysite nanotube-based composite material is dispersed in N,N-dimethylformamide, N,N'-dicyclohexylcarbodiimide and N-hydroxysuccinimide are added, stirred for 2-3 hours, and then polydopamine-modified bimetallic composite nanoparticles are added, the pH of the reaction mixture is adjusted to 5.4-5.6 by a 1 mol / L hydrochloric acid aqueous solution, and the reaction is carried out in a nitrogen atmosphere for 20-30 hours. After the reaction is completed, the solid product is filtered, and the obtained solid product is rinsed with methanol for 10-15 times, and then vacuum dried at 60-70°C for 10-20 hours to obtain an organic-inorganic hybrid composite material; wherein the halloysite nanotube-based composite material The mass ratio of the material, N,N-dimethylformamide, N,N'-dicyclohexylcarbodiimide, N-hydroxysuccinimide, and polydopamine modified bimetallic composite nanoparticles is (5-8): (100-300): (3.2-4.8): (1.6-2.4): (3-5); a 50wt% polyethyleneimine aqueous solution is added to a Tris-HCl buffer solution with a concentration of 10mmol / L and a pH of 8.5, and then the organic-inorganic hybrid composite material is added, and the reaction is carried out at 55-65°C for 2.5-3.5h, and then stirred at room temperature for 12-16h, centrifuged, and the solid product is washed 2-4 times with deionized water and dried to obtain a hydrophilic modified organic-inorganic hybrid nanoparticle. The invention discloses a modified antibacterial and antifungal additive, wherein the amount ratio of polyethyleneimine aqueous solution, Tris-HCl buffer solution and organic-inorganic hybrid composite material is (9-16) g: (150-250) mL: (5-7) g; octadecylamine and ethanol are mixed, and then added into a Tris-HCl buffer solution with a concentration of 10 mmol / L and a pH of 8.5, stirred for 20-40 min, and then the hydrophilic modified organic-inorganic hybrid composite material is added, incubated at 45-55° C. for 10-14 h, centrifuged, and the obtained solid product is washed with deionized water for 2-4 times and dried to obtain a modified antibacterial and antifungal additive; wherein the amount ratio of octadecylamine, ethanol, Tris-HCl buffer solution and hydrophilic modified organic-inorganic hybrid composite material is (9-16) g: (150-250) mL: (5-7) g; octadecylamine and ethanol are mixed, and then added into a Tris-HCl buffer solution with a concentration of 10 mmol / L and a pH of 8.5, stirred for 20-40 min, and then the hydrophilic modified organic-inorganic hybrid composite material is added, and the mixture is incubated at 45-55° C. for 10-14 h, centrifuged, and the obtained solid product is washed with deionized water for 2-4 times and dried to obtain a modified antibacterial and antifungal additive; The dosage ratio of the hybrid composite material is (1.8-3.3) g: (60-100) g: (100-150) mL: (8-10) g; in the above process, the carboxyl groups on the surface of the halloysite nanotube-based composite material undergo amidation reaction with the amino groups on the surface of the polydopamine-modified bimetallic composite nanoparticles, and the polydopamine-modified bimetallic composite nanoparticles are deposited on the halloysite nanotube-based composite material by chemical bond connection to obtain an organic-inorganic hybrid composite material, and the catechol groups in the polydopamine in the organic-inorganic hybrid composite material react with the amino groups in polyethyleneimine and octadecylamine respectively, and hydrophilic and hydrophobic long chains are connected to the surface of the organic-inorganic hybrid composite material to achieve amphiphilicity.
[0014] Preferably, in step (5), the contents of the components in the mildew and anti-slip TPE material are as follows: 45-50 parts of modified SEBS, 8-12 parts of polypropylene, 20-30 parts of white oil, 3-15 parts of modified antibacterial and mildew-proof additives, 1.5-4 parts of nano-silicon dioxide, and 0.2-0.6 parts of antioxidant 1010, by weight; the melt extrusion temperature is 185-200°C; in the above process, the addition of white oil can change the softness and fluidity of the SEBS and polypropylene composite material, play a role in plasticization and softening, and nano-silicon dioxide can improve the hardness and wetting and anti-slip properties of the material; preferably, in step (5), the preparation method of the modified SEBS is:
[0015] Step A1, add SEBS to xylene, stir at 90-100°C for 20-40min, then add maleic anhydride and dibenzoyl peroxide, continue stirring and reacting for 2.5-3.5h, cool to 30-40°C, precipitate the reaction product with ethanol, wash, and dry to obtain maleic anhydride grafted SEBS; wherein the mass ratio of SEBS, xylene, maleic anhydride, and dibenzoyl peroxide is (10-15): (90-170): (2-3): ( 1.1-1.7); In the above process, the double bond in maleic anhydride reacts with SEBS to obtain maleic anhydride grafted SEBS; 2,2-bis[4-(4-aminophenoxy)phenyl]propane is added to dimethyl sulfoxide, hydrochloric acid with a concentration of 36wt% is added, and stirred for 20-30min, and then a dimethyl sulfoxide dispersion of montmorillonite with a concentration of 0.1g / mL is added, and stirred at a speed of 500-700r / min at 75-85°C for 2.5 -3.5h, cooled to room temperature, filtered, the obtained filter residue was added to dimethyl sulfoxide for washing, and continued to stir for 40-80min, and washed repeatedly with dimethyl sulfoxide until no precipitation was produced after adding a 1mol / L silver nitrate aqueous solution, and the final washed product was vacuum dried at 40-60°C for 20-30h, and ground through a 1000-1200 mesh sieve to obtain modified montmorillonite; wherein, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, hydrochloric acid, montmorillonite The amount ratio of the dimethyl sulfoxide dispersion is (12.5-25) g: (10-20) mL: (50-100) mL; in the above process, 2,2-bis[4-(4-aminophenoxy)phenyl]propane reacts with hydrochloric acid to form a quaternary ammonium cation, which is then exchanged with montmorillonite to insert the hard and long-chain 2,2-bis[4-(4-aminophenoxy)phenyl]propane structure into the layer structure of montmorillonite, thereby expanding the interlayer spacing and achieving the exfoliation of the montmorillonite layer structure;
[0016] Step A2, dispersing maleic anhydride grafted SEBS in chloroform, adding modified montmorillonite, stirring at a speed of 200-300 r / min at room temperature for 20-30 hours, evaporating and removing the solvent to obtain modified SEBS; wherein the mass ratio of maleic anhydride grafted SEBS, chloroform, and modified montmorillonite is (10-15): (60-150): (6-12).
[0017] The mildew-proof and anti-slip TPE material is prepared by the method for preparing the mildew-proof and anti-slip TPE material.
[0018] Application of the mildew-proof and anti-slip TPE material in the preparation of toothbrush handles.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The present invention uses a halloysite nanotube-based composite material to react with polydopamine-modified bimetallic composite nanoparticles to obtain an organic-inorganic hybrid composite material. The polydopamine-modified bimetallic composite nanoparticles are obtained by grafting polydopamine with a mesoporous structure on the surface of a titanium dioxide / cuprous oxide heterostructure. The titanium dioxide / cuprous oxide heterostructure can exert excellent antibacterial and mildew-proof properties, and the mesoporous polydopamine can achieve sustained release of the bimetallic composite nanoparticles, and also solve the problems of burst release, instability, and short antibacterial timeliness of cuprous oxide. The present invention grafts and deposits the polydopamine-modified bimetallic composite nanoparticles on a tubular halloysite nanotube-based composite material to increase the halloysite nanotube-based The surface roughness of the composite material is improved to form a tubular organic-inorganic hybrid composite material with a rough surface, which is dispersed in the SEBS substrate to improve the mechanical properties, wear resistance, anti-slip properties and long-lasting antibacterial and anti-mildew properties of the anti-mildew and anti-skid TPE material; further, hydrophilic polyethyleneimine and hydrophobic octadecylamine long chains are chemically grafted on the surface of the organic-inorganic hybrid composite material to improve the amphiphilicity of the organic-inorganic hybrid composite material, so that the anti-mildew and anti-skid TPE material has amphiphilicity, has good binding properties for both dry and wet interfaces, and exhibits better anti-slip properties. In addition, the introduction of polyethyleneimine and octadecylamine can also enhance the compatibility and dispersibility of the organic-inorganic hybrid composite material in the SEBS matrix;
[0021] 2. The present invention obtains a compound essential oil with excellent antibacterial and mildew-proof properties by compounding cinnamon essential oil and cassia twig essential oil. By etching the halloysite nanotubes, the specific surface area and pore volume of the halloysite nanotubes are increased, and the loading amount of the compound essential oil can be increased; by amination and carboxylation of the halloysite nanotubes, chitosan can be grafted on the surface of the halloysite nanotubes, and the compound essential oil in the halloysite nanotubes is encapsulated, so that the compound essential oil is sustained-released, and chitosan itself can also exert an antibacterial effect; and then 2-(ethylene oxide-2-yl)acetic acid is grafted on chitosan to introduce carboxyl groups, so as to provide reactive groups for the deposition of polydopamine-modified bimetallic composite nanoparticles on the halloysite nanotube-based composite material, thereby enhancing the connection strength between the two, thereby further improving the antibacterial and mildew-proof properties of the mildew-proof and anti-slip TPE material;
[0022] 3. In the present invention, montmorillonite is intercalated with 2,2-bis[4-(4-aminophenoxy)phenyl]propane, so that montmorillonite can be more easily and evenly dispersed in the SEBS matrix. The introduction of organic chains makes montmorillonite exhibit organophilicity, thereby improving the compatibility between montmorillonite and SEBS. SEBS is then grafted with maleic anhydride to further increase the compatibility between montmorillonite and SEBS, so that the modified SEBS has excellent thermal stability and mechanical properties, thereby improving the thermal stability and mechanical properties of the mildew-proof and anti-slip TPE material. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a process flow chart of the preparation method of the mildew-proof and anti-slip TPE material of the present invention;
[0024] Figure 2 It is a comparison chart of the antibacterial rate test of Escherichia coli and Staphylococcus aureus of the mildew-proof and anti-slip TPE materials of Examples 2-4 of the present invention and Comparative Examples 1-7;
[0025] Figure 3 It is a comparison chart of tensile strength tests of mildew-proof and anti-slip TPE materials of Examples 2-4 of the present invention and Comparative Examples 1-7;
[0026] Figure 4 It is a comparison chart of the wear volume test of the mildew-proof and anti-slip TPE materials of Examples 2-4 of the present invention and Comparative Examples 1-7;
[0027] Figure 5 It is a comparison chart of the friction coefficient (dry and wet) test of the mildew-proof and anti-slip TPE materials of Examples 2-4 of the present invention and Comparative Examples 1-7. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] This embodiment discloses a method for preparing a modified SEBS, comprising the following steps:
[0031] Step A1, add 12.5g SEBS to 130g xylene, stir at 95°C for 30min, then add 2.5g maleic anhydride and 1.4g dibenzoyl peroxide, continue stirring and reacting for 3h, cool to 35°C, precipitate the reaction product with ethanol, wash, and dry to obtain maleic anhydride grafted SEBS; add 18.8g 2,2-bis[4-(4-aminophenoxy)phenyl]propane to 95g dimethyl sulfoxide, add 15mL 36wt% hydrochloric acid, stir for 25min, and then add 75mL A 0.1 g / mL dimethyl sulfoxide dispersion of montmorillonite was stirred at 80°C and 600 r / min for 3 h, cooled to room temperature, filtered, and the resulting residue was washed with 250 g of dimethyl sulfoxide, stirred for 60 min, and washed repeatedly with dimethyl sulfoxide until no precipitation was produced after adding 1 mol / L silver nitrate aqueous solution. The final washed product was vacuum dried at 50°C for 25 h, ground through a 1200 mesh sieve, and modified montmorillonite was obtained;
[0032] Step A2: 12.5 g of maleic anhydride grafted SEBS was dispersed in 105 g of chloroform, 9 g of modified montmorillonite was added, and the mixture was stirred at a speed of 250 r / min at room temperature for 25 h. The solvent was evaporated to obtain modified SEBS.
[0033] Example 2
[0034] This embodiment discloses a method for preparing a mildew-proof and anti-slip TPE material, comprising the following steps:
[0035] Step (1), at 40°C, dispersing 5g of halloysite nanotubes in 30mL of 5mol / L sulfuric acid aqueous solution, etching for 12h, washing with deionized water and drying to obtain pretreated halloysite nanotubes; dispersing 3g of pretreated halloysite nanotubes in 100g of toluene, ultrasonically treating for 100min, adding 7.5g of 3-aminopropyltriethoxysilane, reflux reacting at 110°C for 12h, centrifuging, washing, and drying to obtain amination halloysite nanotubes; at room temperature, suspending 3g of amination halloysite nanotubes in 300g of N,N-dimethylformamide, adding 40g of succinic anhydride, stirring for 20h, centrifuging, washing, and drying to obtain carboxylated halloysite nanotubes;
[0036] Step (2), mixing cinnamon essential oil and litsea cubeba essential oil in a mass ratio of 50:25 to obtain a compound essential oil; mixing carboxylated halloysite nanotubes, the compound essential oil and water in a mass ratio of 1:2:50, stirring for 20 minutes and then ultrasonically treating for 20 minutes, vacuum loading at 0.01 atm for 30 minutes, returning to atmospheric pressure, repeating the vacuum loading twice, centrifuging, washing and drying to obtain loaded modified halloysite nanotubes;
[0037] Step (3), mixing equal volumes of a chitosan acetic acid dispersion having a concentration of 0.8 wt% and an essential oil-loaded halloysite nanotube aqueous dispersion having a concentration of 1 wt%, stirring at room temperature for 20 h, centrifuging, washing, and drying to obtain chitosan grafted loaded modified halloysite nanotubes; dispersing 4 g of chitosan grafted loaded modified halloysite nanotubes in 150 g of N,N-dimethylformamide, stirring for 20 min, and adding 5 g 2-(2-oxirane-2-yl)acetic acid, stirred at 70°C for 20h, centrifuged, the precipitate obtained by centrifugation was washed with ethanol, water, acetone and then dried to obtain a halloysite nanotube-based composite material; copper nitrate trihydrate, tetrabutyl titanate and ethanol were mixed in a mass ratio of 1:0.5:5, stirred for 10min, stirred at 160°C for 7h, filtered, washed and dried after the reaction was completed to obtain bimetallic composite nanoparticles; 32g ethanol, 45g deionized water, 0.4mL ammonia solution with a concentration of 28wt%, and 3g bimetallic composite nanoparticles were mixed, stirred at room temperature for 20min, and then 15mL dopamine hydrochloride aqueous solution with a concentration of 0.05g / mL was added, stirred for 6h, filtered, washed and dried after the reaction was completed to obtain polydopamine modified bimetallic composite nanoparticles;
[0038] Step (4), dispersing 5g of the halloysite nanotube-based composite material in 100g of N,N-dimethylformamide, adding 3.2g of N,N'-dicyclohexylcarbodiimide and 1.6g of N-hydroxysuccinimide, stirring for 2h, then adding 3g of polydopamine-modified bimetallic composite nanoparticles, adjusting the pH of the reaction mixture to 5.4 with a 1mol / L hydrochloric acid aqueous solution, reacting in a nitrogen atmosphere for 20h, filtering the resulting solid product after washing with methanol 10 times, and vacuum drying at 60°C for 10h to obtain an organic-inorganic hybrid composite material; adding 9g of polyethyleneimine aqueous solution to 150mL of a 10mmol / L Tris-HCl buffer solution with a pH of 8.5, then adding 5g of the organic-inorganic hybrid composite material, and The mixture was reacted at 55-65°C for 2.5 hours, and then stirred at room temperature for 12 hours, centrifuged, and the solid product was washed twice with deionized water and dried to obtain a hydrophilic modified organic-inorganic hybrid composite material; 1.8 g of octadecylamine was mixed with 60 g of ethanol, and then added to 100 mL of Tris-HCl buffer with a concentration of 10 mmol / L and a pH of 8.5, stirred for 20 minutes, and then 8 g of the hydrophilic modified organic-inorganic hybrid composite material was added, incubated at 45°C for 10 hours, centrifuged, and the solid product was washed twice with deionized water and dried to obtain a modified antibacterial and antifungal additive;
[0039] Step (5), 45 parts of modified SEBS, 8 parts of polypropylene, and 20 parts of white oil are mixed, and stirred for 20 minutes, and then 3 parts of modified antibacterial and mildew-proof additives, 1.5 parts of nano-silicon dioxide, and 0.2 parts of antioxidant 1010 are added, and stirring is continued for 10 minutes to obtain a mixture; the mixture is melt-extruded at 185° C., granulated, and cooled to obtain a mildew-proof and anti-slip TPE material.
[0040] Example 3
[0041] This embodiment discloses a method for preparing a mildew-proof and anti-slip TPE material, comprising the following steps:
[0042] Step (1), at 60°C, dispersing 10g of halloysite nanotubes in 50mL of a 5mol / L sulfuric acid aqueous solution, etching for 16h, washing with deionized water and drying to obtain pretreated halloysite nanotubes; dispersing 6g of the pretreated halloysite nanotubes in 200g of toluene, ultrasonically treating for 150min, adding 18.9g of 3-aminopropyltriethoxysilane, reflux reacting at 130°C for 16h, centrifuging, washing, and drying to obtain amination halloysite nanotubes; at room temperature, suspending 6g of amination halloysite nanotubes in 500g of N,N-dimethylformamide, adding 70g of succinic anhydride, stirring for 28h, centrifuging, washing, and drying to obtain carboxylated halloysite nanotubes;
[0043] Step (2), mixing cinnamon essential oil and litsea cubeba essential oil in a mass ratio of 75:50 to obtain a compound essential oil; mixing carboxylated halloysite nanotubes, the compound essential oil and water in a mass ratio of 1:3:80, stirring for 30 minutes and then ultrasonically treating for 30 minutes, vacuum loading at 0.012 atm for 40 minutes, returning to atmospheric pressure, repeating the vacuum loading for 3 times, centrifuging, washing and drying to obtain loaded modified halloysite nanotubes;
[0044] Step (3), mixing equal volumes of a chitosan acetic acid dispersion having a concentration of 1.2 wt% and an essential oil-loaded halloysite nanotube aqueous dispersion having a concentration of 1.5 wt%, stirring at room temperature for 30 h, centrifuging, washing, and drying to obtain chitosan grafted loaded modified halloysite nanotubes; dispersing 6 g of chitosan grafted loaded modified halloysite nanotubes in 300 g of N,N-dimethylformamide, stirring for 40 min, and adding 8 g 2-(2-oxirane-2-yl)acetic acid, stirred at 90°C for 30h, centrifuged, the precipitate obtained by centrifugation was washed with ethanol, water, acetone and then dried to obtain a halloysite nanotube-based composite material; copper nitrate trihydrate, tetrabutyl titanate and ethanol were mixed in a mass ratio of 1:1.2:10, stirred for 30min, stirred at 180°C for 9h, filtered, washed and dried after the reaction was completed to obtain bimetallic composite nanoparticles; 64g ethanol, 90g deionized water, 0.8mL ammonia solution with a concentration of 28wt%, and 8g bimetallic composite nanoparticles were mixed, stirred at room temperature for 40min, and then 25mL dopamine hydrochloride aqueous solution with a concentration of 0.05g / mL was added, stirred for 8h, filtered, washed and dried after the reaction was completed to obtain polydopamine modified bimetallic composite nanoparticles;
[0045] Step (4), dispersing 8g of the halloysite nanotube-based composite material in 300g of N,N-dimethylformamide, adding 4.8g of N,N'-dicyclohexylcarbodiimide and 2.4g of N-hydroxysuccinimide, stirring for 3h, then adding 5g of polydopamine-modified bimetallic composite nanoparticles, adjusting the pH of the reaction mixture to 5.6 with a 1mol / L hydrochloric acid aqueous solution, reacting in a nitrogen atmosphere for 30h, filtering after the reaction, washing the obtained solid product with methanol for 15 times, and vacuum drying at 70°C for 20h to obtain an organic-inorganic hybrid composite material; adding 16g of polyethyleneimine aqueous solution to 250mL of a 10mmol / L Tris-HCl buffer solution with a pH of 8.5, then adding 7g of the organic-inorganic hybrid composite material, The mixture was reacted at 65°C for 3.5 hours, and then stirred at room temperature for 16 hours, centrifuged, and the solid product was washed 4 times with deionized water and dried to obtain a hydrophilic modified organic-inorganic hybrid composite material; 3.3 g of octadecylamine was mixed with 100 g of ethanol, and then added to 150 mL of Tris-HCl buffer with a concentration of 10 mmol / L and a pH of 8.5, stirred for 40 minutes, and then 10 g of the hydrophilic modified organic-inorganic hybrid composite material was added, incubated at 55°C for 14 hours, centrifuged, and the solid product was washed 4 times with deionized water and dried to obtain a modified antibacterial and antifungal additive;
[0046] Step (5), 50 parts of modified SEBS, 12 parts of polypropylene, and 30 parts of white oil are mixed, and stirred for 40 minutes, and then 15 parts of modified antibacterial and mildew-proof additives, 4 parts of nano-silicon dioxide, and 0.6 parts of antioxidant 1010 are added, and stirring is continued for 20 minutes to obtain a mixture; the mixture is melt-extruded at 200° C., granulated, and cooled to obtain a mildew-proof and anti-slip TPE material.
[0047] Example 4
[0048] This embodiment discloses a method for preparing a mildew-proof and anti-slip TPE material, comprising the following steps:
[0049] Step (1), at 50°C, dispersing 7.5g of halloysite nanotubes in 40mL of 5mol / L sulfuric acid aqueous solution, etching for 14h, washing with deionized water and drying to obtain pretreated halloysite nanotubes; dispersing 4.5g of pretreated halloysite nanotubes in 150g of toluene, ultrasonically treating for 120min, adding 13.2g of 3-aminopropyltriethoxysilane, reflux reacting at 120°C for 14h, centrifuging, washing, and drying to obtain amination halloysite nanotubes; at room temperature, suspending 4.5g of amination halloysite nanotubes in 400g of N,N-dimethylformamide, adding 55g of succinic anhydride, stirring for 24h, centrifuging, washing, and drying to obtain carboxylated halloysite nanotubes;
[0050] Step (2), mixing cinnamon essential oil and litsea cubeba essential oil in a mass ratio of 62.5:37.5 to obtain a compound essential oil; mixing carboxylated halloysite nanotubes, the compound essential oil and water in a mass ratio of 1:2.5:65, stirring for 25 minutes and then ultrasonically treating for 25 minutes, vacuum loading at 0.011 atm for 35 minutes, returning to atmospheric pressure, repeating the vacuum loading for 3 times, centrifuging, washing and drying to obtain loaded modified halloysite nanotubes;
[0051] Step (3), mixing equal volumes of a 1wt% chitosan acetic acid dispersion and a 1.2wt% essential oil-loaded halloysite nanotube aqueous dispersion, stirring at room temperature for 25h, centrifuging, washing, and drying to obtain chitosan grafted loaded modified halloysite nanotubes; dispersing 5g of chitosan grafted loaded modified halloysite nanotubes in 250g of N,N-dimethylformamide, stirring for 30min, and adding 6.5g 2-(2-oxirane-2-yl)acetic acid, stirred at 80°C for 25h, centrifuged, the precipitate obtained by centrifugation was washed with ethanol, water, acetone and then dried to obtain a halloysite nanotube-based composite material; copper nitrate trihydrate, tetrabutyl titanate and ethanol were mixed in a mass ratio of 1:0.8:7.5, stirred for 20min, stirred at 170°C for 8h, filtered, washed and dried after the reaction was completed to obtain bimetallic composite nanoparticles; 48g ethanol, 67.5g deionized water, 0.6mL ammonia solution with a concentration of 28wt%, and 5.5g bimetallic composite nanoparticles were mixed, stirred at room temperature for 30min, and then 20mL dopamine hydrochloride aqueous solution with a concentration of 0.05g / mL was added, stirred for 7h, filtered, washed and dried after the reaction was completed to obtain polydopamine modified bimetallic composite nanoparticles;
[0052] Step (4), dispersing 6.5g of the halloysite nanotube-based composite material in 200g of N,N-dimethylformamide, adding 4g of N,N'-dicyclohexylcarbodiimide and 2g of N-hydroxysuccinimide, stirring for 2.5h, then adding 4g of polydopamine-modified bimetallic composite nanoparticles, adjusting the pH of the reaction mixture to 5.5 with a 1mol / L hydrochloric acid aqueous solution, reacting in a nitrogen atmosphere for 25h, filtering after the reaction, washing the obtained solid product with methanol 13 times, and vacuum drying at 65°C for 15h to obtain an organic-inorganic hybrid composite material; adding 12.5g of polyethyleneimine aqueous solution to 200mL of a 10mmol / L Tris-HCl buffer solution with a pH of 8.5, then adding 6g of the organic-inorganic hybrid composite; The composite material was reacted at 60°C for 3h, then stirred at room temperature for 14h, centrifuged, and the obtained solid product was washed 3 times with deionized water and dried to obtain a hydrophilic modified organic-inorganic hybrid composite material; 2.6g of octadecylamine was mixed with 80g of ethanol, and then added to 125mL of Tris-HCl buffer with a concentration of 10mmol / L and a pH of 8.5, stirred for 30min, and then 9g of the hydrophilic modified organic-inorganic hybrid composite material was added, incubated at 50°C for 12h, centrifuged, and the obtained solid product was washed 3 times with deionized water and dried to obtain a modified antibacterial and antifungal additive;
[0053] Step (5), 47.5 parts of modified SEBS, 10 parts of polypropylene, and 25 parts of white oil are mixed, and stirred for 30 minutes, and then 9 parts of modified antibacterial and mildew-proof additives, 2.7 parts of nano-silicon dioxide, and 0.4 parts of antioxidant 1010 are added, and stirring is continued for 15 minutes to obtain a mixture; the mixture is melt-extruded at 190° C., granulated, and cooled to obtain a mildew-proof and anti-slip TPE material.
[0054] The modified SEBS used in the above Examples 2-4 is the modified SEBS prepared in Example 1.
[0055] Comparative Example 1
[0056] Compared with Example 4, in the process of preparing the mildew-proof and anti-slip TPE material in Comparative Example 1, maleic anhydride-grafted SEBS was used instead of modified SEBS, and other conditions remained unchanged.
[0057] Comparative Example 2
[0058] Compared with Example 4, in the process of preparing the organic-inorganic hybrid composite material in Comparative Example 2, the loaded modified halloysite nanotubes are used instead of the halloysite nanotube-based composite material, and other conditions remain unchanged.
[0059] Comparative Example 3
[0060] Compared with Example 4, in the process of preparing the bimetallic composite nanoparticles in Comparative Example 3, copper nitrate trihydrate was not added, that is, the synthesized titanium dioxide nanoparticles were used instead of the bimetallic composite nanoparticles, and other conditions remained unchanged.
[0061] Comparative Example 4
[0062] Compared with Example 4, in the process of preparing the bimetallic composite nanoparticles in Comparative Example 4, tetrabutyl titanate was not added, that is, the synthesized cuprous oxide nanoparticles were used instead of the bimetallic composite nanoparticles, and other conditions remained unchanged.
[0063] Comparative Example 5
[0064] Compared with Example 4, in the process of preparing the modified antibacterial and mildew-proof additive in Comparative Example 5, polydopamine-modified bimetallic composite nanoparticles are used instead of the organic-inorganic hybrid composite material, and other conditions remain unchanged.
[0065] Comparative Example 6
[0066] Compared with Example 4, in the process of preparing the loaded modified halloysite nanotubes in Comparative Example 5, cinnamon essential oil was not added, and other conditions remained unchanged.
[0067] Comparative Example 7
[0068] Compared with Example 4, in the process of preparing the loaded modified halloysite nanotubes in Comparative Example 7, no litsea cubeba essential oil was added, and other conditions remained unchanged.
[0069] In the above embodiments and comparative examples, the outer diameter of the halloysite nanotube is 10-50 nm, the inner diameter is 5-20 nm, and the length is 0.5-3 μm, which is from Angxing New Carbon Material Changzhou Co., Ltd.; chitosan, with a molecular weight of 190000-310000 Da, a viscosity of 200-800 cPs, and a deacetylation degree of 75%-85%, is from Sigma-Aldrich; cinnamon essential oil, with a content of ≥99%, model D1UL, item number 9957, is from Kunshan Shengan Biotechnology Co., Ltd.; Litsea cubeba essential oil, a light yellow clear liquid, with a content of ≥99%, is from Wuhan Huaxiang Kejie Biotechnology Co., Ltd.; Polyethyleneimine aqueous solution, concentration 50%, molecular weight 70,000, from Jinjinle Chemical Co., Ltd.; antioxidant 1010, active ingredient content 99.8%, powder appearance, model 1010, pH value 5.0-7.0, from Dongguan Xingyuan Chemical Co., Ltd.; SEBS, brand G1654, brand American Kraton, density / specific gravity 0.918g / cm³, polystyrene content 29-32%, from Dongguan Canhui New Material Technology Co., Ltd.; polypropylene, density 0.90-0.91g / cm3, tensile strength 70MPa, brand 8511E, from Dongguan Changping Senhai Plastic Trading Co., Ltd.
[0070] Experimental example
[0071] The performance tests were performed on the mildew and anti-slip TPE materials prepared in Examples 2-4 and Comparative Examples 1-7.
[0072] 1. Mechanical properties test: The tensile strength is tested in accordance with GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber".
[0073] 2. Antibacterial performance test: Tested in accordance with JIS Z2801-2012, the test bacteria are Escherichia coli ATCC 25922 and Staphylococcus aureus ATCC 6538P.
[0074] 3. Anti-mildew performance test: Tested in accordance with JIS Z2911-2018, the test fungi used are Aspergillus niger ATCC 6275, Penicillium pinophilum ATCC 36839, Paecilomyces variotii ATCC 18502, Trichoderma viride ATCC 9645 and Chaetomium globosum ATCC6205.
[0075] 4. Anti-slip performance test: Refer to standard GB / T 3903.6-2005 to conduct dry and wet friction static friction coefficient test to characterize the anti-slip performance.
[0076] 5. Wear resistance test: The wear resistance is measured using an Akron abrasion machine.
[0077] The test results are shown in Table 1:
[0078]
[0079] It can be seen from the test results in Table 1 that the mildew-proof and anti-slip TPE materials prepared in Examples 2-4 of the present invention have excellent mechanical strength, toughness, wear resistance, anti-slip properties and long-lasting antibacterial and mildew-proof properties.
[0080] Analysis of antibacterial and mildew proof properties: From the comparison of comparative examples 2-7 with example 4, it can be seen that chitosan, cuprous oxide, titanium dioxide, cinnamon essential oil, and Litsea cubeba essential oil have different antibacterial and mildew proof mechanisms, which have different degrees of influence on the antibacterial and mildew proof properties of the materials. In addition, from comparative examples 2 and 5, it can be seen that chitosan is grafted on the loaded modified halloysite nanotubes to achieve the sustained release of the compound essential oil, thereby achieving a lasting antibacterial and mildew proof effect. From the comparison of comparative example 4 with example 4, it can be seen that nano titanium dioxide not only can exert antibacterial and mildew proof properties itself, but also has a certain effect on the sustained release of cuprous oxide, thereby affecting the antibacterial and mildew proof properties of the material.
[0081] Analysis of mechanical properties and wear resistance: From the comparison between comparative example 1 and example 4, it can be seen that the intercalation modification of montmorillonite makes it easier to evenly disperse montmorillonite in the SEBS matrix, and the introduction of organic chains makes montmorillonite exhibit organophilicity, thereby improving the compatibility between montmorillonite and SEBS, thereby improving the mechanical properties and wear resistance of the mildew-proof and anti-slip TPE material; from the comparison between comparative example 5 and example 4, it can be seen that the halloysite nanotube-based composite material in the organic-inorganic hybrid composite material, with inorganic halloysite nanotubes as the base material, can increase the thermal stability and mechanical properties of SEBS, thereby improving the mechanical properties and wear resistance of the mildew-proof and anti-slip TPE material.
[0082] Anti-slip analysis: From the comparison between comparative example 1 and embodiment 4, it can be seen that due to the layer structure of montmorillonite, although the mechanical properties and wear resistance of the mildew-proof and anti-slip TPE material are improved, its anti-slip performance will have a certain negative impact; from the comparison between comparative examples 6-7 and embodiment 4, it can be seen that due to the lubricating effect of cinnamon essential oil and Litsea cubeba essential oil as essential oils themselves, the anti-slip performance of the mildew-proof and anti-slip TPE material will also have a certain degree of adverse effect; from the comparison between comparative example 5 and embodiment 4, it can be seen that the long tube rod structure of the halloysite nanotube-based composite material in the organic-inorganic hybrid composite material can increase the surface roughness of the material, and the inorganic hard structure can pierce the water film, further improve the friction coefficient, and improve the dry and wet anti-slip performance.
[0083] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a mildew-proof and anti-slip TPE material, characterized in that: The following steps are involved: Step (1), etching, amino modification, and carboxyl modification are performed on the halloysite nanotubes in sequence to obtain carboxylated halloysite nanotubes; Step (2), loading the compound essential oil into the carboxylated halloysite nanotubes to obtain loaded modified halloysite nanotubes; The compound essential oil is obtained by mixing cinnamon essential oil and litsea cubeba essential oil in a mass ratio of (50-75):(25-50); Step (3), first modifying the loaded modified halloysite nanotubes with chitosan, and then treating them with 2-(2-oxirane-1-yl)acetic acid to obtain a halloysite nanotube-based composite material, the specific method is as follows: Mix equal volumes of a chitosan acetic acid dispersion having a concentration of 0.8-1.2wt% and an essential oil-loaded halloysite nanotube aqueous dispersion having a concentration of 1-1.5wt%, stir at room temperature for 20-30h, centrifuge, wash, and dry to obtain chitosan grafted loaded modified halloysite nanotubes; disperse the chitosan grafted loaded modified halloysite nanotubes in N,N-dimethylformamide, stir for 20-40min, add 2-(2-oxirane-1)acetic acid, stir and react at 70-90°C for 20-30h, centrifuge, wash the precipitate obtained by centrifugation with ethanol, water, and acetone, and then dry to obtain a halloysite nanotube-based composite material, wherein the mass ratio of the chitosan grafted loaded modified halloysite nanotubes, N,N-dimethylformamide, and 2-(2-oxirane-1)acetic acid is (4-6):(150-300):(5-8); Copper nitrate trihydrate and tetrabutyl titanate are used as raw materials to prepare bimetallic composite nanoparticles, which are then modified by polydopamine to obtain polydopamine-modified bimetallic composite nanoparticles. The specific method is as follows: Copper nitrate trihydrate, tetrabutyl titanate, and ethanol are mixed in a mass ratio of 1:(0.5-1.2):(5-10), stirred for 10-30 minutes, stirred and reacted at 160-180°C for 7-9 hours, filtered, washed, and dried after the reaction to obtain bimetallic composite nanoparticles; ethanol, deionized water, an ammonia solution with a concentration of 28wt%, and bimetallic composite nanoparticles are mixed, stirred at room temperature for 20-40 minutes, and then a dopamine hydrochloride aqueous solution with a concentration of 0.05g / mL is added, stirred and reacted for 6-8 hours, filtered, washed, and dried after the reaction to obtain polydopamine modified bimetallic composite nanoparticles, wherein the amount ratio of ethanol, deionized water, ammonia solution, bimetallic composite nanoparticles, and dopamine hydrochloride aqueous solution is: (32-64)g:(45-90)g:(0.4-0.8)mL:(3-8)g:(15-25)mL; Step (4), the halloysite nanotube-based composite material reacts with polydopamine-modified bimetallic composite nanoparticles to obtain an organic-inorganic hybrid composite material, and polyethyleneimine and octadecylamine are grafted on the surface of the organic-inorganic hybrid composite material to obtain a modified antibacterial and antifungal additive. The specific method is as follows: The halloysite nanotube-based composite material is dispersed in N,N-dimethylformamide, N,N'-dicyclohexylcarbodiimide and N-hydroxysuccinimide are added, stirred for 2-3 hours, and then polydopamine-modified bimetallic composite nanoparticles are added, and the pH of the reaction mixture is adjusted to 5.4-5.6 by a 1 mol / L hydrochloric acid aqueous solution, and the reaction is carried out in a nitrogen atmosphere for 20-30 hours. After the reaction is completed, the solid product is filtered, and the obtained solid product is rinsed with methanol for 10-15 times, and then vacuum dried at 60-70°C for 10-20 hours to obtain an organic-inorganic hybrid composite material; wherein the mass ratio of the halloysite nanotube-based composite material, N,N-dimethylformamide, N,N'-dicyclohexylcarbodiimide, N-hydroxysuccinimide, and polydopamine-modified bimetallic composite nanoparticles is (5-8):(100-300):(3.2-4.8):(1.6-2.4):(3-5); A 50 wt% polyethyleneimine aqueous solution is added to a 10 mmol / L Tris-HCl buffer solution with a pH of 8.5, and then the organic-inorganic hybrid composite material is added, and the mixture is reacted at 55-65° C. for 2.5-3.5 hours, and then stirred at room temperature for 12-16 hours, centrifuged, and the obtained solid product is washed with deionized water for 2-4 times, and dried to obtain a hydrophilic modified organic-inorganic hybrid composite material, wherein the amount ratio of the polyethyleneimine aqueous solution, the Tris-HCl buffer solution, and the organic-inorganic hybrid composite material is (9-16) g:(150-250) mL:(5-7) g; Octadecylamine and ethanol are mixed, and then added to a Tris-HCl buffer solution with a concentration of 10 mmol / L and a pH of 8.5, stirred for 20-40 minutes, and then a hydrophilic modified organic-inorganic hybrid composite material is added, incubated at 45-55° C. for 10-14 hours, centrifuged, and the obtained solid product is washed with deionized water for 2-4 times and dried to obtain a modified antibacterial and mildew-proof additive; wherein the amount ratio of octadecylamine, ethanol, Tris-HCl buffer solution, and hydrophilic modified organic-inorganic hybrid composite material is (1.8-3.3) g: (60-100) g: (100-150) mL: (8-10) g; Step (5), mixing modified SEBS, polypropylene and white oil, and then adding modified antibacterial and mildew-proof additives, nano-silicon dioxide and antioxidant 1010 to obtain a mixture; melt-extruding the mixture, granulating, and cooling to obtain a mildew-proof and anti-slip TPE material; Wherein, the preparation method of the modified SEBS comprises the following steps: Step A1, adding SEBS to xylene, stirring at 90-100°C for 20-40min, then adding maleic anhydride and dibenzoyl peroxide, stirring and reacting for 2.5-3.5h, cooling to 30-40°C, precipitating the reaction product with ethanol, washing, and drying to obtain maleic anhydride grafted SEBS; wherein the mass ratio of SEBS, xylene, maleic anhydride, and dibenzoyl peroxide is (10-15):(90-170):(2-3):(1.1-1.7); Add 2,2-bis[4-(4-aminophenoxy)phenyl]propane to dimethyl sulfoxide, add 36wt% hydrochloric acid, stir for 20-30min, then add 0.1g / mL montmorillonite in dimethyl sulfoxide dispersion, stir at 75-85℃ and 500-700r / min for 2.5-3.5h, cool to room temperature, filter, add the obtained filter residue to dimethyl sulfoxide for washing, continue stirring for 40-80min, repeat with The product is washed with dimethyl sulfoxide until no precipitation is produced after adding a silver nitrate aqueous solution with a concentration of 1 mol / L, and the final washed product is vacuum dried at 40-60° C. for 20-30 hours, and ground through a 1000-1200 mesh sieve to obtain a modified montmorillonite; wherein the amount ratio of 2,2-bis[4-(4-aminophenoxy)phenyl]propane, hydrochloric acid, and dimethyl sulfoxide dispersion of montmorillonite is (12.5-25) g:(10-20) mL:(50-100) mL; Step A2, dispersing maleic anhydride grafted SEBS in chloroform, adding modified montmorillonite, stirring at a speed of 200-300 r / min at room temperature for 20-30 hours, evaporating and removing the solvent to obtain modified SEBS; wherein the mass ratio of maleic anhydride grafted SEBS, chloroform, and modified montmorillonite is (10-15):(60-150):(6-12).
2. The method for preparing the mildew-proof and anti-slip TPE material according to claim 1, characterized in that: In the step (1), the preparation method of the carboxylated halloysite nanotubes comprises: dispersing the halloysite nanotubes in a 5 mol / L sulfuric acid aqueous solution at 40-60° C. and etching for 12-16 hours, washing with deionized water and drying to obtain pretreated halloysite nanotubes; wherein the ratio of the halloysite nanotubes to the sulfuric acid aqueous solution is (5-10) g: (30-50) mL; The pretreated halloysite nanotubes are dispersed in toluene, ultrasonically treated for 100-150 minutes, and then 3-aminopropyltriethoxysilane is added, refluxed at 110-130° C. for 12-16 hours, centrifuged, washed, and dried to obtain amination halloysite nanotubes; wherein the mass ratio of the pretreated halloysite nanotubes, toluene, and 3-aminopropyltriethoxysilane is (3-6):(100-200):(7.5-18.9); At room temperature, the aminated halloysite nanotubes are suspended in N,N-dimethylformamide, and succinic anhydride is added, stirred for reaction for 20-28 hours, centrifuged, washed, and dried to obtain carboxylated halloysite nanotubes; wherein the mass ratio of the aminated halloysite nanotubes, N,N-dimethylformamide, and succinic anhydride is (3-6):(300-500):(40-70).
3. The method for preparing the mildew-proof and anti-slip TPE material according to claim 1, characterized in that: In the step (2), the compound essential oil loading method is as follows: carboxylated halloysite nanotubes, compound essential oil and water are mixed in a mass ratio of 1:(2-3):(50-80), stirred for 20-30 minutes and then ultrasonically treated for 20-30 minutes, vacuum loaded at 0.01-0.012 atm for 30-40 minutes, restored to atmospheric pressure, repeated the vacuum loading 2-3 times, centrifuged, washed and dried.
4. The method for preparing the mildew-proof and anti-slip TPE material according to claim 1, characterized in that: In the step (5), the contents of the components in the mildew and anti-slip TPE material are, by weight: 45-50 parts of modified SEBS, 8-12 parts of polypropylene, 20-30 parts of white oil, 3-15 parts of modified antibacterial and mildew-proof additives, 1.5-4 parts of nano-silicon dioxide, and 0.2-0.6 parts of antioxidant 1010; the melt extrusion temperature is 185-200°C.
5. A mildew-proof and anti-slip TPE material prepared by the method for preparing the mildew-proof and anti-slip TPE material according to any one of claims 1 to 4.
6. Use of the mildew-proof and anti-slip TPE material according to claim 5 in the preparation of a toothbrush handle.