A method for preparing a flame retardant polylactic acid composite material

By modifying the chemical reaction of aluminum diethylphosphinate with ethylenediaminetetraacetic acid, cyclodextrin and sodium hypophosphite, a stable inclusion compound was formed, and the compatibility of aluminum diethylphosphinate with polymer was solved. The problem of poor performance improves the flame retardant performance and stability of polylactic acid composite materials, and achieves the improvement of the environmental protection of the materials.

CN118515958BActive Publication Date: 2024-11-19JIANGSU HENGLI CHEM FIBER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410985731.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-19
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

In the prior art, the compatibility and interfacial adhesion of aluminum diethylphosphinate with polymers are poor, resulting in a decrease in the mechanical properties and flame retardant properties of the materials, and the commonly used modification methods are complex or have environmental problems.

Method used

Using the chemical reaction of modified aluminum diethylphosphinate with ethylenediaminetetraacetic acid, cyclodextrin and sodium hypophosphite, the aluminum diethylphosphinate was coated with cyclodextrin through chelation and esterification reaction. Inside, a stable inclusion compound is formed to improve its compatibility and stability with polylactic acid.

Benefits of technology

It significantly improves the compatibility and stability of modified aluminum diethylphosphinate and polylactic acid, ensures that it is uniformly dispersed in polylactic acid composite materials, enhances flame retardant properties and avoids the reduction of the mechanical properties of the materials. At the same time, it adopts The natural cyclic oligosaccharide compound cyclodextrin improves the environmental protection of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118515958B_ABST
    Figure CN118515958B_ABST
Patent Text Reader

Abstract

The invention relates to a method for preparing a flame-retardant polylactic acid composite material. The flame-retardant polylactic acid masterbatch is cast in a flat vulcanizer to obtain the flame-retardant polylactic acid composite material. The flame-retardant polylactic acid masterbatch is obtained by melt blending and extruding a modified aluminum diethylphosphinate flame retardant and a polylactic acid masterbatch in sequence; the preparation method of the modified aluminum diethylphosphinate flame retardant is as follows: aluminum diethylphosphinate and ethylenediaminetetraacetic acid are added to distilled water for uniform dispersion, reacted at 60-70°C, then cyclodextrin and sodium hypophosphite are added, the temperature is raised to 70-80°C for further reaction, and after the reaction is completed, the distilled water is reduced in pressure and distilled to 1 / 4-1 / 3 of the remaining distilled water, and then the product is dried, washed and dried in sequence to obtain the modified aluminum diethylphosphinate flame retardant. The invention fixes aluminum diethylphosphinate in the internal cavity of cyclodextrin by physical and chemical bonding, improves its compatibility and stability with polylactic acid, and improves the flame retardant performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardant materials and relates to a method for preparing a flame retardant polylactic acid composite material. Background Art

[0002] Polylactic acid is a biodegradable bio-based polyester that can be made from starch. Due to its excellent physical and mechanical properties, it has potential application value in the fields of electronics, automobiles, packaging, etc. However, since pure polylactic acid is flammable and produces a large number of flammable droplets during combustion, its application is limited. Therefore, it is of great significance to improve the flame retardant properties of polylactic acid materials.

[0003] Aluminum diethylphosphinate is a safe and efficient phosphorus-based flame retardant, and is also the main component of the intumescent halogen-free flame retardant system. It is widely used in the halogen-free flame retardant modification process of various high-value-added engineering plastics. However, aluminum diethylphosphinate and related flame retardant synergists (such as nitrogen-based flame retardants and carbon-forming agents) are often powders. During the application process, there are problems such as poor compatibility, poor dispersibility, and poor adhesion to the interface of the modified polymer, which leads to a decrease in the mechanical properties and flame retardant properties of the material.

[0004] Based on these problems, the prior art usually performs surface modification on aluminum diethylphosphinate to improve its compatibility and interfacial adhesion with polymers. For example, invention patent CN113817229A discloses an anti-migration modified aluminum diethylphosphinate, a preparation method and its application. The surface of aluminum diethylphosphinate is modified by a double treatment method of pyrophosphate coating treatment and surface coupling treatment with a silane coupling agent to obtain anti-migration modified aluminum diethylphosphinate, and is used to improve the flame retardant properties of high molecular polymers such as nylon and glass fiber reinforced nylon, TPU, PBT, epoxy resin, and unsaturated resin. Invention patent CN110591341A discloses a halogen-free flame retardant synergistic functional masterbatch for nylon resin modification and a preparation method thereof. Aluminum diethylphosphinate is treated with aluminum sol, zinc oxide sol, phytic acid, zinc ion doped aluminum hydroxide, and zirconium hydrogen phosphate powder through a multi-step reaction to obtain a multi-composite inorganic material coated aluminum diethylphosphinate, and finally a nylon masterbatch with flame retardant function is obtained. However, the anti-migration modified aluminum diethylphosphite prepared by CN113817229A and the multiple composite inorganic material coated aluminum diethylphosphite prepared by CN110591341A still show the characteristics of inorganic materials, and their compatibility and interfacial adhesion with high molecular polymer materials are still very poor. In addition, CN110591341A uses a variety of inorganic and organic materials to treat aluminum diethylphosphite, and the preparation method is complicated.

[0005] In addition, the literature (Research on the Application of Aluminum Diethylphosphinate and Its Microcapsules in Rigid Polyurethane Foam [C]. / / Proceedings of the 8th National Conference on Fire Safety Materials. 2017: 156-157.) modified aluminum diethylphosphinate with melamine formaldehyde resin to obtain flame-retardant microcapsules, which were used to improve the flame retardant properties of rigid polyurethane foam. However, melamine formaldehyde resin is a non-environmentally friendly resin material and there is a problem of formaldehyde release during use.

[0006] In summary, currently, the modified material and aluminum diethylphosphinate are coated mainly through physical action, and the compatibility between the two is also poor, with defects such as low coating efficiency and instability. In addition, with the continuous improvement of human environmental awareness, the use of natural polymer materials to prepare aluminum diethylphosphinate flame retardants has become a current research hotspot.

[0007] Therefore, it is of great significance to study a method for preparing a flame retardant polylactic acid composite material to solve the problems existing in the prior art. Summary of the invention

[0008] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for preparing a flame retardant polylactic acid composite material.

[0009] To achieve the above object, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing a flame-retardant polylactic acid composite material, wherein the flame-retardant polylactic acid masterbatch is cast in a flat vulcanizer to obtain the flame-retardant polylactic acid composite material, and the flame-retardant polylactic acid masterbatch is obtained by sequentially melt-blending a modified diethyl aluminum phosphinate flame retardant and the polylactic acid masterbatch and extruding and granulating.

[0011] The preparation method of the modified aluminum diethylphosphinate flame retardant is as follows: aluminum diethylphosphinate and ethylenediaminetetraacetic acid are added into distilled water and uniformly dispersed, and reacted at 60-70°C, wherein the increase of reaction temperature is helpful to improve molecular motion and promote the chelation of ethylenediaminetetraacetic acid and aluminum diethylphosphinate, but it is wasted if the temperature is too high; then cyclodextrin and sodium hypophosphite are added, and the temperature is raised to 70-80°C to continue the reaction, wherein the temperature is raised from 60-70°C to 70-80°C to help improve the molecular motion of aluminum diethylphosphinate and enter the cavity of cyclodextrin, but it is wasted if the temperature is too high; after the reaction is completed, the reduced pressure distillation is performed until 1 / 4-1 / 3 of the distilled water remains, which is helpful to create a humid environment and promote the reaction between ethylenediaminetetraacetic acid and cyclodextrin in the subsequent high-temperature drying process; and then the product is dried, washed and dried in sequence to obtain the modified aluminum diethylphosphinate flame retardant.

[0012] As the preferred technical solution:

[0013] In the method for preparing a flame-retardant polylactic acid composite material as described above, the pressure of the flat vulcanizer is 10-20 MPa, and the tableting temperature is 180-190°C.

[0014] In the method for preparing a flame-retardant polylactic acid composite material as described above, the modified aluminum diethylphosphinate flame retardant and the polylactic acid masterbatch are dried separately before melt blending to ensure that the final moisture content of the polylactic acid masterbatch and the modified aluminum diethylphosphinate flame retardant is less than 250 ppm;

[0015] The drying temperature of the modified diethylphosphinate aluminum flame retardant is 100~120℃, and the drying time is 3~5h;

[0016] The drying temperature of polylactic acid masterbatch is 100~120℃, and the drying time is 3~5h.

[0017] In the method for preparing a flame-retardant polylactic acid composite material as described above, the dosage of the modified diethyl aluminum phosphinate flame retardant is 15-20wt% of the polylactic acid masterbatch; the higher the dosage of the modified diethyl aluminum phosphinate flame retardant, the better the flame retardant effect, but too high a dosage will result in waste.

[0018] In the method for preparing a flame-retardant polylactic acid composite material as described above, melt blending is performed in a twin-screw extruder, and the processing temperature of the twin-screw extruder is 170-190° C. If the processing temperature is too low, the modified aluminum diethylphosphinate flame retardant and the polylactic acid masterbatch cannot be mixed evenly, which is not conducive to granulation; if the processing temperature is too high, energy waste will be caused. Within the temperature range of the present invention, uniform flame-retardant polylactic acid masterbatch can be smoothly prepared.

[0019] According to the preparation method of a flame-retardant polylactic acid composite material as described above, the molar ratio of aluminum diethylphosphinate to ethylenediaminetetraacetic acid is 1:2-4, the aluminum salt in aluminum diethylphosphinate can be chelated with ethylenediaminetetraacetic acid, so that ethylenediaminetetraacetic acid is coated on the surface of aluminum diethylphosphinate powder, and the ethylenediaminetetraacetic acid is excessive to ensure sufficient chelation; the dosage ratio of aluminum diethylphosphinate to distilled water is 1g:3-5mL, the molar ratio of cyclodextrin to aluminum diethylphosphinate is 1:1-2, and theoretically each cyclodextrin can coat multiple aluminum diethylphosphinates. In the present invention, cyclodextrin can coat 2 aluminum diethylphosphinates, and a slight excess of cyclodextrin is helpful for coating aluminum diethylphosphinate, but too high a cyclodextrin is wasteful, resulting in low coating efficiency; the molar ratio of sodium hypophosphite to aluminum diethylphosphinate is 1-1.5:1.

[0020] In the method for preparing a flame-retardant polylactic acid composite material as described above, the reaction time is 40 to 60 minutes before adding cyclodextrin and sodium hypophosphite;

[0021] After adding cyclodextrin and sodium hypophosphite, the reaction time is 2 to 3 hours.

[0022] In the method for preparing a flame-retardant polylactic acid composite material as described above, the pressure of the reduced pressure distillation is 35-45 kPa and the temperature is 40-50°C.

[0023] As described above, the preparation method of a flame-retardant polylactic acid composite material has a drying temperature of 140-160°C and a drying time of 1-2h, and the temperature increase helps to promote the esterification reaction between ethylenediaminetetraacetic acid and cyclodextrin; washing refers to washing with ethanol for 3 times, and the ratio of ethanol to product in each washing is 10-15mL:1g; the drying temperature is 70-90°C, and the drying time is 30-50min, and the ethanol is evaporated to obtain a modified diethyl aluminum phosphinate flame retardant.

[0024] A method for preparing a flame-retardant polylactic acid composite material as described in any of the above items, wherein the flame-retardant polylactic acid composite material has a flame-retardant grade of V0 after a UL-94 vertical burning test, and no droplets are generated in the UL-94 vertical burning test (the flame-retardant grade of the non-flame-retardant polylactic acid composite material is NR, with severe droplets and poor flame retardant properties);

[0025] The tensile strength of the flame retardant polylactic acid composite material is not less than 40MPa (the tensile strength of the non-flame retardant polylactic acid composite material is 54MPa).

[0026] The principle of the present invention is:

[0027] Aluminum diethylphosphinate can chelate with ethylenediaminetetraacetic acid, so that ethylenediaminetetraacetic acid can be stably coated on the surface of aluminum diethylphosphinate particles through coordination bonds.

[0028] Cyclodextrin is a molecule with an internal cavity structure. It can encapsulate aluminum diethylphosphinate in the interior by physical coating to form an inclusion complex. Under the condition of sodium hypophosphite as a catalyst, the alcohol hydroxyl group in the cyclodextrin molecule and the carboxyl group of ethylenediaminetetraacetic acid on the surface of aluminum diethylphosphinate undergo esterification reaction. This chemical reaction further strengthens the bond between aluminum diethylphosphinate and cyclodextrin, and fixes aluminum diethylphosphinate in the internal cavity of cyclodextrin by forming an ester bond. This bonding method not only includes physical coating, but also involves chemical bonding, which greatly improves the stability of the inclusion complex.

[0029] Through this combination of physical and chemical bonding, cyclodextrin can effectively encapsulate aluminum diethylphosphinate in its internal cavity. The two have good compatibility and stable bonding, and aluminum diethylphosphinate particles are not easy to diffuse out of the cyclodextrin, thus ensuring the stability of the encapsulation.

[0030] Cyclodextrin is a natural cyclic oligosaccharide compound with good compatibility with starch-based polylactic acid. Aluminum diethylphosphinate coated with cyclodextrin has good stability in polylactic acid composites. Aluminum diethylphosphinate does not directly contact the polylactic acid composite and can be well dispersed in the polylactic acid composite. It is not easy to migrate and precipitate, and has little effect on the mechanical properties of the flame-retardant polylactic acid composite.

[0031] In addition, cyclodextrin as a polysaccharide compound is an efficient carbon-forming agent. The presence of nitrogen-containing groups in the ethylenediaminetetraacetic acid molecule allows it to be used as a gas source and organically combined with the diethylphosphinate aluminum acid source to form an intumescent flame retardant system; the cyclodextrin-coated diethylphosphinate aluminum flame retardant can produce intumescent residual carbon during the combustion process, effectively improving the flame retardant properties of the polylactic acid material.

[0032] Beneficial effects:

[0033] (1) A method for preparing a flame-retardant polylactic acid composite material of the present invention, in which, under the condition of sodium hypophosphite as a catalyst, the alcohol hydroxyl groups in the cyclodextrin molecules react with the carboxyl groups of ethylenediaminetetraacetic acid on the surface of aluminum diethylphosphinate to undergo an esterification reaction, thereby fixing aluminum diethylphosphinate in the internal cavity of the cyclodextrin, thereby improving the compatibility and stability of the modified aluminum diethylphosphinate flame retardant with polylactic acid;

[0034] (2) A method for preparing a flame-retardant polylactic acid composite material of the present invention, wherein cyclodextrin is a natural cyclic oligosaccharide compound and has good compatibility with starch-based polylactic acid, and diethylaluminum phosphinate coated with cyclodextrin has good stability in the polylactic acid composite material; the cyclodextrin-coated diethylaluminum phosphinate flame retardant can produce expanded carbon residue during combustion, thereby effectively improving the flame retardant properties of the flame-retardant polylactic acid material. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic diagram of the structure of the modified diethyl aluminum phosphinate flame retardant of the present invention. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0037] The test methods involved in the performance indicators in the embodiments and comparative examples of the present invention are as follows:

[0038] UL94 vertical burning test: the slice specimen size is 130 mm × 13 mm × 3.2 mm;

[0039] Tensile strength: tested according to GB / T 1040.2-2022, the slice specimen size is 130 mm × 100 mm × 3.2 mm.

[0040] The β-cyclodextrin of the present invention comes from McLean (product number: C804562); the polylactic acid comes from McLean (Mw ~110,000).

[0041] Example 1

[0042] A method for preparing a flame retardant polylactic acid composite material, the specific steps are as follows:

[0043] (1) Aluminum diethylphosphinate and ethylenediaminetetraacetic acid were added to distilled water and dispersed uniformly, and reacted at 70°C for 40 min. Then, β-cyclodextrin and sodium hypophosphite were added, and the temperature was raised to 80°C and the reaction was continued for 2 h. After the reaction, the product was distilled under reduced pressure at a pressure of 45 kPa and a temperature of 50°C until the remaining distilled water was 1 / 4. Then, the product was dried at 160°C for 1 h, and then washed with ethanol for 3 times. The ratio of ethanol to product in each washing was 15 mL: 1 g. Finally, it was dried at 90°C for 30 min to obtain a product with the structure shown in Figure 1 The modified aluminum diethylphosphinate flame retardant shown;

[0044] Wherein, the molar ratio of aluminum diethylphosphinate to ethylenediaminetetraacetic acid is 1:3, the dosage ratio of aluminum diethylphosphinate to distilled water is 1 g:4 mL, the molar ratio of β-cyclodextrin to aluminum diethylphosphinate is 1:1.5, and the molar ratio of sodium hypophosphite to aluminum diethylphosphinate is 1.4:1;

[0045] (2) drying the modified aluminum diethylphosphinate flame retardant at 110°C for 4 hours, and drying the polylactic acid masterbatch at 110°C for 4 hours;

[0046] (3) melt-blending the modified aluminum diethylphosphinate flame retardant dried in step (2) with polylactic acid masterbatch in a twin-screw extruder at a processing temperature of 180° C., and then extruding and granulating to obtain flame-retardant polylactic acid masterbatch;

[0047] Among them, the amount of modified diethylphosphinate aluminum flame retardant is 18wt% of the polylactic acid masterbatch;

[0048] (4) The flame retardant polylactic acid masterbatch was cast in a flat vulcanizer at a pressure of 15 MPa and a tableting temperature of 190°C to obtain a flame retardant polylactic acid composite material.

[0049] The flame retardant grade of the finally prepared flame retardant polylactic acid composite material is V0 after the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test; the tensile strength of the flame retardant polylactic acid composite material is 42MPa.

[0050] Comparative Example 1

[0051] A method for preparing a flame-retardant polylactic acid composite material is basically the same as that of Example 1, except that ethylenediaminetetraacetic acid is omitted in step (1).

[0052] The flame retardant grade of the finally prepared flame retardant polylactic acid composite material is V1 after the UL-94 vertical burning test, and molten droplets are generated in the UL-94 vertical burning test; the tensile strength of the flame retardant polylactic acid composite material is 39 MPa.

[0053] By comparing Comparative Example 1 with Example 1, it can be found that the flame retardant properties of the flame retardant polylactic acid composite material of Comparative Example 1 are slightly worse, and its tensile strength decreases. This is because the binding performance of diethyl aluminum phosphinate that has not been modified with ethylenediaminetetraacetic acid and cyclodextrin is poor, and cyclodextrin cannot well coat diethyl aluminum phosphinate. Therefore, the dispersion performance of diethyl aluminum phosphinate in polylactic acid is reduced, a small amount of molten droplets are generated, the flame retardant properties are deteriorated, and the mechanical properties are deteriorated.

[0054] Example 2

[0055] A method for preparing a flame retardant polylactic acid composite material, the specific steps are as follows:

[0056] (1) Add aluminum diethylphosphinate and ethylenediaminetetraacetic acid to distilled water and disperse them uniformly, react at 65°C for 50 minutes, then add β-cyclodextrin and sodium hypophosphite, raise the temperature to 75°C and continue the reaction for 2.5 hours, and after the reaction, decompress and distill at 40 kPa and 45°C until the remaining 1 / 3 of the distilled water, then dry the product at 150°C for 1.5 hours, and then wash it with ethanol for 3 times, the ratio of ethanol to product in each washing is 12 mL: 1 g, and finally dry it at 80°C for 40 minutes to obtain a modified aluminum diethylphosphinate flame retardant;

[0057] Among them, the molar ratio of diethylaluminum phosphinate to ethylenediaminetetraacetic acid is 1:2.5, the dosage ratio of diethylaluminum phosphinate to distilled water is 1g:3.5mL, the molar ratio of β-cyclodextrin to diethylaluminum phosphinate is 1:1.3, and the molar ratio of sodium hypophosphite to diethylaluminum phosphinate is 1.2:1;

[0058] (2) drying the modified aluminum diethylphosphinate flame retardant at 105°C for 4.5 hours, and drying the polylactic acid masterbatch at 105°C for 4.5 hours;

[0059] (3) melt-blending the modified aluminum diethylphosphinate flame retardant dried in step (2) with polylactic acid masterbatch in a twin-screw extruder at a processing temperature of 175° C., and then extruding and granulating to obtain flame-retardant polylactic acid masterbatch;

[0060] Among them, the amount of modified diethylphosphinate aluminum flame retardant is 16wt% of the polylactic acid masterbatch;

[0061] (4) The flame retardant polylactic acid masterbatch was cast in a flat vulcanizer at a pressure of 13 MPa and a tableting temperature of 185°C to obtain a flame retardant polylactic acid composite material.

[0062] The flame retardant grade of the finally prepared flame retardant polylactic acid composite material is V0 after the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test; the tensile strength of the flame retardant polylactic acid composite material is 43MPa.

[0063] Example 3

[0064] A method for preparing a flame retardant polylactic acid composite material, the specific steps are as follows:

[0065] (1) Add aluminum diethylphosphinate and ethylenediaminetetraacetic acid to distilled water and disperse them uniformly, react at 60°C for 60 minutes, then add β-cyclodextrin and sodium hypophosphite, raise the temperature to 70°C and continue to react for 3 hours, and after the reaction, decompress and distill at a pressure of 35 kPa and a temperature of 40°C until the remaining 1 / 4 of the distilled water is left, then dry the product at 140°C for 2 hours, and then wash it with ethanol for 3 times, the ratio of ethanol to product in each washing is 10 mL: 1 g, and finally dry it at 70°C for 50 minutes to obtain a modified aluminum diethylphosphinate flame retardant;

[0066] Wherein, the molar ratio of aluminum diethylphosphinate to ethylenediaminetetraacetic acid is 1:2, the dosage ratio of aluminum diethylphosphinate to distilled water is 1 g:3 mL, the molar ratio of β-cyclodextrin to aluminum diethylphosphinate is 1:1, and the molar ratio of sodium hypophosphite to aluminum diethylphosphinate is 1:1;

[0067] (2) drying the modified aluminum diethylphosphinate flame retardant at 100°C for 5 hours, and drying the polylactic acid masterbatch at 100°C for 5 hours;

[0068] (3) melt-blending the modified aluminum diethylphosphinate flame retardant dried in step (2) with polylactic acid masterbatch in a twin-screw extruder at a processing temperature of 170° C., and then extruding and granulating to obtain flame-retardant polylactic acid masterbatch;

[0069] Among them, the amount of modified diethylphosphinate aluminum flame retardant is 15wt% of the polylactic acid masterbatch;

[0070] (4) The flame retardant polylactic acid masterbatch was cast in a flat plate vulcanizer at a pressure of 10 MPa and a tableting temperature of 180°C to obtain a flame retardant polylactic acid composite material.

[0071] The flame retardant grade of the finally prepared flame retardant polylactic acid composite material is V0 after the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test; the tensile strength of the flame retardant polylactic acid composite material is 45MPa.

[0072] Example 4

[0073] A method for preparing a flame retardant polylactic acid composite material, the specific steps are as follows:

[0074] (1) Add aluminum diethylphosphinate and ethylenediaminetetraacetic acid to distilled water and disperse them uniformly, react at 65°C for 50 minutes, then add β-cyclodextrin and sodium hypophosphite, raise the temperature to 75°C and continue the reaction for 2.5 hours, and after the reaction, decompress and distill at 40 kPa and 45°C until the remaining 1 / 3 of the distilled water is left, then dry the product at 145°C for 1.75 hours, and then wash it with ethanol for 3 times, with the ratio of ethanol to product in each washing being 13 mL:1 g, and finally dry it at 75°C for 45 minutes to obtain a modified aluminum diethylphosphinate flame retardant;

[0075] Among them, the molar ratio of diethylaluminum phosphinate to ethylenediaminetetraacetic acid is 1:3.5, the dosage ratio of diethylaluminum phosphinate to distilled water is 1g:4.5mL, the molar ratio of β-cyclodextrin to diethylaluminum phosphinate is 1:1.8, and the molar ratio of sodium hypophosphite to diethylaluminum phosphinate is 1.5:1;

[0076] (2) drying the modified aluminum diethylphosphinate flame retardant at 115°C for 3.5 hours, and drying the polylactic acid masterbatch at 115°C for 3.5 hours;

[0077] (3) melt-blending the modified aluminum diethylphosphinate flame retardant dried in step (2) with polylactic acid masterbatch in a twin-screw extruder at a processing temperature of 185° C., and then extruding and granulating to obtain flame-retardant polylactic acid masterbatch;

[0078] Among them, the amount of modified diethylphosphinate aluminum flame retardant is 19wt% of the polylactic acid masterbatch;

[0079] (4) The flame retardant polylactic acid masterbatch was cast in a flat vulcanizer at a pressure of 18 MPa and a tabletting temperature of 185°C to obtain a flame retardant polylactic acid composite material.

[0080] The flame retardant grade of the finally prepared flame retardant polylactic acid composite material is V0 after the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test; the tensile strength of the flame retardant polylactic acid composite material is 41MPa.

[0081] Example 5

[0082] A method for preparing a flame retardant polylactic acid composite material, the specific steps are as follows:

[0083] (1) Add aluminum diethylphosphinate and ethylenediaminetetraacetic acid to distilled water and disperse them uniformly, react at 60°C for 60 minutes, then add β-cyclodextrin and sodium hypophosphite, raise the temperature to 70°C and continue to react for 3 hours, and after the reaction, decompress and distill at a pressure of 35 kPa and a temperature of 40°C until the remaining amount of distilled water is 1 / 4, then dry the product at 155°C for 1.25 hours, and then wash it with ethanol for 3 times, the ratio of ethanol to product in each washing is 10 mL: 1 g, and finally dry it at 85°C for 35 minutes to obtain a modified aluminum diethylphosphinate flame retardant;

[0084] The molar ratio of aluminum diethylphosphinate to ethylenediaminetetraacetic acid is 1:4, the dosage ratio of aluminum diethylphosphinate to distilled water is 1 g:5 mL, the molar ratio of β-cyclodextrin to aluminum diethylphosphinate is 1:2, and the molar ratio of sodium hypophosphite to aluminum diethylphosphinate is 1.3:1;

[0085] (2) drying the modified aluminum diethylphosphinate flame retardant at 120°C for 3 hours, and drying the polylactic acid masterbatch at 120°C for 3 hours;

[0086] (3) melt-blending the modified aluminum diethylphosphinate flame retardant dried in step (2) with polylactic acid masterbatch in a twin-screw extruder at a processing temperature of 190° C., and then extruding and granulating to obtain flame-retardant polylactic acid masterbatch;

[0087] Among them, the amount of modified diethylphosphinate aluminum flame retardant is 20wt% of the polylactic acid masterbatch;

[0088] (4) The flame retardant polylactic acid masterbatch was cast in a flat plate vulcanizer at a pressure of 20 MPa and a tabletting temperature of 180°C to obtain a flame retardant polylactic acid composite material.

[0089] The flame retardant grade of the finally prepared flame retardant polylactic acid composite material is V0 after the UL-94 vertical burning test, and no molten droplets are generated in the UL-94 vertical burning test; the tensile strength of the flame retardant polylactic acid composite material is 40MPa.

Claims

1. A method for preparing a flame retardant polylactic acid composite material, wherein the flame retardant polylactic acid masterbatch is cast in a flat vulcanizer to obtain a flame retardant polylactic acid composite material, characterized in that: The flame retardant polylactic acid masterbatch is obtained by melt blending and extruding the modified aluminum diethylphosphinate flame retardant and the polylactic acid masterbatch in sequence; The preparation method of the modified diethyl phosphinate aluminum flame retardant is as follows: diethyl phosphinate aluminum and ethylenediaminetetraacetic acid are added into distilled water and uniformly dispersed, reacted at 60-70°C, then cyclodextrin and sodium hypophosphite are added, the temperature is raised to 70-80°C to continue the reaction, and after the reaction is completed, the distillation is carried out under reduced pressure until 1 / 4-1 / 3 of the distilled water remains, and then the product is dried, washed and dried in sequence to obtain the modified diethyl phosphinate aluminum flame retardant.

2. The method for preparing a flame retardant polylactic acid composite material according to claim 1, characterized in that: The pressure of the flat plate vulcanizer is 10~20MPa, and the tableting temperature is 180~190℃.

3. The method for preparing a flame retardant polylactic acid composite material according to claim 1, characterized in that: The modified aluminum diethylphosphinate flame retardant and the polylactic acid masterbatch are dried separately before melt blending; The drying temperature of the modified diethylphosphinate aluminum flame retardant is 100~120℃, and the drying time is 3~5h; The drying temperature of polylactic acid masterbatch is 100~120℃, and the drying time is 3~5h.

4. The method for preparing a flame retardant polylactic acid composite material according to claim 1, characterized in that: The dosage of modified diethyl phosphinate aluminum flame retardant is 15-20wt% of the polylactic acid masterbatch.

5. The method for preparing a flame retardant polylactic acid composite material according to claim 1, characterized in that: The melt blending is carried out in a twin-screw extruder, and the processing temperature of the twin-screw extruder is 170~190℃.

6. The method for preparing a flame retardant polylactic acid composite material according to claim 1, characterized in that: The molar ratio of aluminum diethylphosphinate to ethylenediaminetetraacetic acid is 1:2-4, the dosage ratio of aluminum diethylphosphinate to distilled water is 1g:3-5mL, the molar ratio of cyclodextrin to aluminum diethylphosphinate is 1:1-2, and the molar ratio of sodium hypophosphite to aluminum diethylphosphinate is 1-1.5:

1.

7. The method for preparing a flame retardant polylactic acid composite material according to claim 1, characterized in that: Before adding cyclodextrin and sodium hypophosphite, the reaction time is 40-60 min; After adding cyclodextrin and sodium hypophosphite, the reaction time is 2 to 3 hours.

8. The method for preparing a flame-retardant polylactic acid composite material according to claim 1, characterized in that: The pressure of vacuum distillation is 35~45kPa and the temperature is 40~50℃.

9. The method for preparing a flame retardant polylactic acid composite material according to claim 1, characterized in that: The drying temperature is 140~160℃ and the drying time is 1~2h; Washing means washing with ethanol for 3 times, and the ratio of ethanol to product in each washing is 10-15 mL:1 g; The drying temperature is 70~90℃ and the drying time is 30~50min.

10. The method for preparing a flame-retardant polylactic acid composite material according to any one of claims 1 to 9, characterized in that: The flame retardant grade of the flame retardant polylactic acid composite material is V0 after the UL-94 vertical burning test, and no droplets are generated in the UL-94 vertical burning test; The tensile strength of the flame retardant polylactic acid composite material is not less than 40MPa.