A method for preparing an acid absorbent for EVA film
By preparing nano-dual mesoporous magnesium oxide and a micellar solution wrapped with magnesium hydroxide, the problem of easy expansion and poor dispersion of active magnesium oxide in EVA film is solved, the water absorption and bonding properties are improved, and the extrusion flow is maintained. The properties and thickness uniformity enhance the bonding strength to the glass.
Patent Information
- Application Number
- CN202410985766.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-23
AI Technical Summary
Activated magnesium oxide easily swells in the EVA film and the particle size is small, resulting in poor dispersion, which affects extrusion fluidity and light transmittance, and refining the activated magnesium oxide will reduce the bonding performance.
The steps of light burning, hydration, filtration, one-time mixing, hydrothermal treatment and calcination are used to prepare nano-double mesoporous magnesium oxide, and a micellar solution wrapping magnesium hydroxide is added to improve the activity and dispersion of magnesium oxide through template agent and hydrothermal treatment. properties, forming a nano-double mesoporous structure to improve water absorption and bonding properties.
The prepared acid absorbent is not easy to expand after absorbing water, improves the bonding performance and light transmittance of the EVA film, maintains extrusion fluidity and thickness uniformity, and enhances the bonding strength to glass.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium oxide acid absorbers, and in particular to a method for preparing an acid absorber for an EVA adhesive film. Background Art
[0002] EVA (polyethylene-vinyl acetate copolymer) film is a thermosetting and sticky film used to be placed between laminated glass. Due to its superiority in adhesion, durability, optical properties, etc., EVA film is increasingly widely used in current components and various optical products, among which one of the most widely used products of EVA film is photovoltaic cells.
[0003] EVA film can cover the surface of photovoltaic cells to form a protective film, thereby protecting the photovoltaic cells from the influence of the external environment and improving the stability and durability of photovoltaic cells. In order to absorb moisture and harmful substances inside the photovoltaic cells, acid absorbers need to be added. At present, the commonly used acid absorber in EVA film is magnesium oxide.
[0004] The mechanism of action of the acid absorber magnesium oxide is to absorb acidic substances through adsorption capacity and undergo oxidation reaction with the acidic substances to generate corresponding oxides. Therefore, the acid absorber magnesium oxide should have strong adsorption capacity and oxidizability.
[0005] Active magnesium oxide has a large specific surface area, and during the preparation process, many defects and lattice distortions will appear on the surface of active magnesium oxide, resulting in unsaturated surface valence bonds. Therefore, it has extremely high chemical activity and physical adsorption capacity. Active magnesium oxide also has high dispersibility. Therefore, the acid absorbent magnesium oxide currently used is mainly active magnesium oxide.
[0006] However, the following problems were found when active magnesium oxide was used as an acid absorber in EVA film: active magnesium oxide easily swells after absorbing water, causing deformation of the EVA film; active magnesium oxide is irregular particles or flaky crystals with an uneven surface. After being added to the EVA film, it can improve the bonding performance of the EVA film, but it will affect the fluidity of the EVA film during extrusion, resulting in uneven thickness of the extruded EVA film.
[0007] The most commonly used solutions to the above problems are: in order to solve the problem that active magnesium oxide is easy to swell after absorbing water, calcium and aluminum elements are added during the preparation of active magnesium oxide to obtain active magnesium oxide containing calcium oxide and aluminum oxide, but this method will affect the activity of the active magnesium oxide; in order to solve the problem that active magnesium oxide affects the fluidity of EVA film during extrusion, the active magnesium oxide is refined to reduce the particle size of the active magnesium oxide, but the smaller the particle size, the easier it is to agglomerate, and the worse the dispersibility in the EVA film, which will affect the light transmittance of the EVA film and also affect the bonding performance of the EVA film. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention provides a method for preparing an acid absorber for EVA film. The prepared acid absorber for EVA film is not easy to swell after absorbing water, has high activity, and will not affect the fluidity, light transmittance and bonding performance of the EVA film during extrusion.
[0009] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:
[0010] A method for preparing an acid absorbent for EVA film, comprising the following steps: light burning, hydration, filtration, primary mixing, secondary mixing, and calcination;
[0011] The light burning is to crush and grind the magnesite to a particle size of 200-300 mesh, then calcine it, and then naturally cool it to 200-250° C. to obtain light-burned magnesium oxide powder;
[0012] The magnesium oxide content of the magnesite is 44.7%;
[0013] In the light calcination, the calcination temperature is 800-900°C and the calcination time is 1.5-2h;
[0014] The hydration comprises mixing the light-burned magnesium oxide powder with water, stirring at a stirring speed of 50-100 rpm for 30-40 minutes, and then ball milling and heating and stirring to obtain a hydrated slurry;
[0015] In the hydration, the mass volume ratio of light-burned magnesium oxide powder to water is 500-550g:3500-4000mL;
[0016] The ball-to-material ratio during the ball milling is 4-5:1, the rotation speed is 350-400rpm, and the time is 40-60min;
[0017] The temperature during the heating and stirring is 90-120°C, the rotation speed is 100-200rpm, and the time is 3-4h;
[0018] The filtering comprises filtering the hydrated slurry using a filter screen with a mesh size of 60-80, removing the filter residue, and obtaining the filtered hydrated slurry;
[0019] The primary mixing comprises mixing the filtered hydrated slurry with the magnesium oxide nanoparticles, stirring at a stirring speed of 100-200 rpm for 30-40 min, and then ball milling to obtain a mixed slurry;
[0020] In the primary mixing, the mass volume ratio of the filtered hydrated slurry to the magnesium oxide nanoparticles is 3000-3500 mL:14-15 g;
[0021] The ball-to-material ratio during ball milling is 10-13:1, the rotation speed is 350-400 rpm, and the time is 40-60 min;
[0022] The method for preparing magnesium oxide nanoparticles comprises the following steps: preparing a first mixed solution, preparing a second mixed solution, and hydrothermally treating;
[0023] The first mixed solution is prepared by mixing magnesium chloride hexahydrate with water, stirring at a stirring speed of 100-200 rpm for 30-40 minutes, adding a template F127 aqueous solution, continuing to stir for 30-40 minutes, and dripping a sodium hydroxide aqueous solution. After the dripping is completed, stirring is continued for 10-20 minutes to obtain a first mixed solution;
[0024] In the preparation of the first mixed solution, the mass volume ratio of magnesium chloride hexahydrate, water, template agent F127 aqueous solution, and sodium hydroxide aqueous solution is 32-35g:120-150mL:250-300mL:90-100mL;
[0025] The mass concentration of the template F127 aqueous solution is 4%;
[0026] The mass concentration of the sodium hydroxide aqueous solution is 20%;
[0027] The dropping speed of the sodium hydroxide aqueous solution is 5-6 mL / min;
[0028] The second mixed solution is prepared by mixing magnesium chloride hexahydrate with water, stirring at a stirring speed of 100-200 rpm for 30-40 min, adding an aqueous solution of sodium dodecylbenzenesulfonate, continuing to stir for 30-40 min, and dripping an aqueous solution of sodium hydroxide. After the dripping is completed, stirring is continued for 10-20 min to obtain a second mixed solution;
[0029] In the preparation of the second mixed solution, the mass volume ratio of magnesium chloride hexahydrate, water, sodium dodecylbenzenesulfonate aqueous solution, and sodium hydroxide aqueous solution is 32-35g:120-150mL:370-400mL:100-120mL;
[0030] The mass concentration of the sodium dodecylbenzenesulfonate aqueous solution is 1%;
[0031] The mass concentration of the sodium hydroxide aqueous solution is 20%;
[0032] The dropping speed of the sodium hydroxide aqueous solution is 5-6 mL / min;
[0033] The hydrothermal treatment comprises adding the first mixed solution and the second mixed solution into a high-pressure reactor, sealing the high-pressure reactor, controlling the temperature of the high-pressure reactor to 110-120° C., standing for 45-50 hours, naturally cooling to room temperature, and then centrifuging, controlling the speed of the centrifugation to be 9000-10000 rpm, and the time to be 10-15 minutes. After washing the precipitate with water, vacuum drying at 70-80° C., and then calcining to obtain magnesium oxide nanoparticles;
[0034] In the hydrothermal treatment, the volume ratio of the first mixed liquid to the second mixed liquid is 140-150:100-110;
[0035] The calcination temperature is 500-550°C and the calcination time is 3.5-4h;
[0036] The secondary mixing is to take the mixed slurry and perform primary drying, then mix it with the micelle solution encapsulating magnesium hydroxide, then perform ball milling, and then perform secondary drying to obtain a mixed powder;
[0037] In the secondary mixing, the volume ratio of the mixed slurry to the micelle solution encapsulating magnesium hydroxide is 2900-3200:140-150;
[0038] The primary drying temperature is 120-140°C and the time is 17-20h;
[0039] The ball-to-material ratio during the ball milling is 10-13:1, the rotation speed is 350-400 rpm, and the time is 4-4.5 hours;
[0040] The secondary drying temperature is 120-140°C and the time is 13-15h;
[0041] The preparation method of the micellar solution encapsulating magnesium hydroxide is as follows: after concentrated hydrochloric acid and anhydrous ethanol are mixed, stirring is carried out at 30-40° C. and a stirring speed of 300-400 rpm for 30-40 min, then citric acid, template F127, and magnesium chloride hexahydrate are added, stirring is continued for 1-1.5 h, and then the mixture is added into a high-pressure reactor, the high-pressure reactor is sealed, the temperature of the high-pressure reactor is controlled to 80-90° C., the mixture is allowed to stand for 25-30 h, and naturally cooled to room temperature to obtain a micellar solution encapsulating magnesium hydroxide;
[0042] In the preparation of the micellar solution encapsulating magnesium hydroxide, the mass volume ratio of concentrated hydrochloric acid, anhydrous ethanol, citric acid, template F127, and magnesium chloride hexahydrate is 6-7 mL: 90-100 mL: 2.5-3 g: 16-18 g: 9-10 g;
[0043] The mass concentration of the concentrated hydrochloric acid is 36%;
[0044] The calcining is to calcine the mixed powder to obtain an acid absorbent for EVA film;
[0045] During the calcination, the calcination temperature is 500-550° C. and the calcination time is 4-4.5 hours.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] (1) The method for preparing the acid absorbent for EVA film of the present invention comprises adding magnesium oxide nanoparticles and a micelle solution encapsulating magnesium hydroxide during the preparation. The preparation method of magnesium oxide nanoparticles is as follows: using templates with different molecular weights, namely template F127 and sodium dodecylbenzene sulfonate, respectively, and then mixing and hydrothermally treating, obtaining magnesium hydroxide containing different templates in the hydrothermal treatment process, and then calcining, during which the template is thermally decomposed to obtain nanometer double mesoporous magnesium oxide with different pore sizes, and then mixing the nanometer double mesoporous magnesium oxide with the hydrated slurry and ball milling, and magnesium hydroxide is attached to the surface of the nanometer double mesoporous magnesium oxide and the pores with large pore sizes, and forming magnesium hydroxide powder with nanometer double mesoporous magnesium oxide as the skeleton in the drying process, and in the sintering process, the nanometer double mesoporous magnesium oxide can play a role in heat dissipation, promote the calcination of magnesium hydroxide, further increase the surface defects and lattice distortion, thereby improving the activity of the generated active magnesium oxide, and the presence of the pore size in the nanometer double mesoporous magnesium oxide can not only increase the specific surface area of the generated active magnesium oxide, but also play a role in water storage, avoiding the problem of easy expansion of the active magnesium oxide after absorbing water; with the improvement of the activity of the active magnesium oxide, the active magnesium oxide is more easily expanded than the active magnesium oxide in the EVA film. The bonding force between the A resin is increased, thereby improving the bonding performance of the EVA film; the preparation method of the micellar solution encapsulating magnesium hydroxide is to mix an inorganic acid, an organic acid, a template agent F127, and magnesium chloride hexahydrate, and then perform a solvent heat treatment to generate magnesium hydroxide, thereby forming a micellar solution encapsulating magnesium hydroxide, wherein the template agent F127 plays the role of a surfactant, and after the micellar solution encapsulating magnesium hydroxide is mixed with the dried magnesium hydroxide powder, the combination of the template agent F127 and the magnesium hydroxide is adsorbed on the surface of the dried magnesium hydroxide powder, and then after drying and calcining, the template agent F127 is thermally decomposed, causing defects and lattice distortion on the surface of magnesium oxide, and the magnesium hydroxide combined with the template agent F127 is dehydrated to nano magnesium oxide, which is combined with the surface of the generated active magnesium oxide, thereby improving the specific surface area, activity, and fluidity of the generated active magnesium oxide, and can also avoid the agglomeration of the active magnesium oxide, improve the bonding force between the active magnesium oxide and the EVA resin in the EVA film, thereby improving the light transmittance and bonding performance of the EVA film, and avoiding the influence on the thickness uniformity of the EVA film;
[0048] (2) The method for preparing the acid absorbent for EVA film of the present invention, wherein the prepared acid absorbent for EVA film is not easy to swell after absorbing water;
[0049] (3) The method for preparing the acid absorbent for EVA film of the present invention has high activity and a specific surface area of 145.1-147.8 m 2 / g, citric acid value (CAA value) is 13-14s, and iodine absorption value is 170.4-173.9mgI2 / gMgO;
[0050] (4) The method for preparing the acid absorber for EVA film of the present invention. The prepared acid absorber for EVA film will not affect the fluidity, light transmittance and bonding performance of the EVA film during extrusion. The average thickness uniformity of the EVA film prepared by the acid absorber for EVA film of the present invention is 0.8-1.0%, the light transmittance is 93.4-93.7%, and the bonding strength to glass is 67-70N / cm. DETAILED DESCRIPTION
[0051] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, the specific implementation methods of the present invention are now described.
[0052] Example 1
[0053] A method for preparing an acid absorbent for EVA film, specifically comprising:
[0054] 1. Light calcination: crush and grind the magnesite to a particle size of 200 mesh, then calcine it at a temperature of 800°C for 1.5 hours, and then naturally cool it to 200°C to obtain light calcined magnesium oxide powder;
[0055] The mass content of magnesium oxide in the magnesite is 44.7%;
[0056] 2. Hydration: Take 500g of light-burned magnesium oxide powder and mix it with 3500mL of water, stir it at a stirring speed of 50rpm for 30min, then ball mill it, control the ball-to-material ratio during ball milling to be 4:1, the speed to be 350rpm, the time to be 40min, then heat and stir it, control the temperature during heating and stirring to be 90℃, the speed to be 100rpm, the time to be 3h, and obtain a hydrated slurry;
[0057] 3. Filtration: Filter the hydrated slurry using a 60-mesh filter to remove the filter residue to obtain the filtered hydrated slurry;
[0058] 4. Primary mixing: 3000 mL of the filtered hydrated slurry was mixed with 14 g of magnesium oxide nanoparticles, stirred at a stirring speed of 100 rpm for 30 min, and then ball milled, with the ball-to-material ratio during ball milling controlled at 10:1, the rotation speed at 350 rpm, and the time at 40 min to obtain a mixed slurry;
[0059] The preparation method of the magnesium oxide nanoparticles is:
[0060] (1) Preparing the first mixed solution: Mix 32 g of magnesium chloride hexahydrate with 120 mL of water, stir at a stirring speed of 100 rpm for 30 min, add 250 mL of a 4% aqueous solution of the template F127, continue stirring for 30 min, dropwise add 90 mL of a 20% aqueous solution of sodium hydroxide, control the dropping speed to 5 mL / min, and continue stirring for 10 min after the addition is completed to obtain the first mixed solution;
[0061] (2) preparing a second mixed solution: mixing 32 g of magnesium chloride hexahydrate with 120 mL of water, stirring at a stirring speed of 100 rpm for 30 min, adding 370 mL of a 1% sodium dodecylbenzene sulfonate aqueous solution, continuing to stir for 30 min, and dripping 100 mL of a 20% sodium hydroxide aqueous solution at a dripping speed of 5 mL / min. After the dripping is completed, stirring is continued for 10 min to obtain a second mixed solution;
[0062] (3) Hydrothermal treatment: 140 mL of the first mixed solution and 100 mL of the second mixed solution were added to a high-pressure reactor. After the high-pressure reactor was sealed, the temperature of the high-pressure reactor was controlled to 110° C., and the reactor was allowed to stand for 45 h, and then naturally cooled to room temperature, and then centrifuged at a speed of 9000 rpm for 10 min. After washing the precipitate with water, the precipitate was vacuum dried at 70° C., and then calcined at a temperature of 500° C. for 3.5 h to obtain magnesium oxide nanoparticles.
[0063] 5. Secondary mixing: Take 2900 mL of the mixed slurry and dry it, control the temperature during drying to be 120°C, and the time is 17 hours, then mix it with 140 mL of the micelle solution encapsulating magnesium hydroxide and perform ball milling, control the ball-to-material ratio during ball milling to be 10:1, the rotation speed to be 350 rpm, and the time to be 4 hours, and then dry it, control the temperature during drying to be 120°C, and the time to be 13 hours to obtain a mixed powder;
[0064] The preparation method of the micellar solution encapsulating magnesium hydroxide is as follows: 6 mL of concentrated hydrochloric acid with a mass concentration of 36% and 90 mL of anhydrous ethanol are mixed, and the mixture is stirred at 30° C. and 300 rpm for 30 min, and then 2.5 g of citric acid, 16 g of template F127, and 9 g of magnesium chloride hexahydrate are added, and the stirring is continued for 1 h, and then the mixture is added into a high-pressure reactor, and the temperature of the high-pressure reactor is controlled to 80° C. after the high-pressure reactor is sealed, and the mixture is allowed to stand for 25 h, and then naturally cooled to room temperature to obtain a micellar solution encapsulating magnesium hydroxide;
[0065] 6. Calcination: Calcinate the mixed powder, control the calcination temperature to 500°C, and the calcination time to 4 hours to obtain an acid absorbent for EVA film.
[0066] The mass content of magnesium oxide in the acid absorber for EVA film obtained in this embodiment is 88.9%.
[0067] Example 2
[0068] A method for preparing an acid absorbent for EVA film, specifically comprising:
[0069] 1. Light calcination: crush and grind the magnesite to a particle size of 200 mesh, then calcine it at a temperature of 850°C for 1.5 hours, and then naturally cool it to 220°C to obtain light calcined magnesium oxide powder;
[0070] The mass content of magnesium oxide in the magnesite is 44.7%;
[0071] 2. Hydration: 520 g of light-burned magnesium oxide powder was mixed with 3800 mL of water, stirred at a stirring speed of 50 rpm for 35 min, and then ball milled, with the ball-to-material ratio during ball milling controlled at 4:1, the rotation speed at 350 rpm, and the time at 50 min. Then, heating and stirring were performed, with the temperature during heating and stirring controlled at 100 ° C, the rotation speed at 150 rpm, and the time at 3.5 h to obtain a hydrated slurry;
[0072] 3. Filtration: Filter the hydrated slurry using a 60-mesh filter to remove the filter residue to obtain the filtered hydrated slurry;
[0073] 4. Primary mixing: 3200 mL of the filtered hydrated slurry was mixed with 14.5 g of magnesium oxide nanoparticles, stirred at a stirring speed of 150 rpm for 35 min, and then ball milled. The ball-to-material ratio during ball milling was controlled to be 12:1, the rotation speed was 350 rpm, and the time was 50 min to obtain a mixed slurry;
[0074] The preparation method of the magnesium oxide nanoparticles is:
[0075] (1) Preparing the first mixed solution: 34 g of magnesium chloride hexahydrate was mixed with 130 mL of water, and the mixture was stirred at a stirring speed of 150 rpm for 35 min. 280 mL of a 4% aqueous solution of the template F127 was added, and the mixture was stirred for 35 min. 95 mL of a 20% aqueous solution of sodium hydroxide was added dropwise at a dropping speed of 5 mL / min. After the addition was completed, the mixture was stirred for 15 min to obtain the first mixed solution.
[0076] (2) preparing a second mixed solution: mixing 34 g of magnesium chloride hexahydrate with 130 mL of water, stirring at a stirring speed of 150 rpm for 35 min, adding 380 mL of a 1% sodium dodecylbenzene sulfonate aqueous solution, continuing to stir for 35 min, and dripping 110 mL of a 20% sodium hydroxide aqueous solution at a dripping speed of 5 mL / min. After the dripping is completed, stirring is continued for 15 min to obtain a second mixed solution;
[0077] (3) Hydrothermal treatment: 145 mL of the first mixed solution and 105 mL of the second mixed solution were added to a high-pressure reactor. After the high-pressure reactor was sealed, the temperature of the high-pressure reactor was controlled to 115°C, and the reactor was allowed to stand for 48 hours, and then naturally cooled to room temperature, and then centrifuged at a speed of 9500 rpm for 12 minutes. After washing the precipitate with water, the precipitate was vacuum dried at 75°C, and then calcined at a temperature of 520°C for 3.5 hours to obtain magnesium oxide nanoparticles.
[0078] 5. Secondary mixing: 3000 mL of the mixed slurry was dried at a temperature of 130°C for 18 h, then mixed with 145 mL of a micellar solution containing magnesium hydroxide and ball milled at a ball-to-material ratio of 12:1, a rotation speed of 350 rpm, and a time of 4 h, and then dried at a temperature of 130°C for 14 h to obtain a mixed powder;
[0079] The preparation method of the micellar solution encapsulating magnesium hydroxide is as follows: 6 mL of concentrated hydrochloric acid with a mass concentration of 36% and 95 mL of anhydrous ethanol are mixed, and the mixture is stirred at 35° C. and 350 rpm for 35 min, and then 2.8 g of citric acid, 17 g of template F127, and 9.5 g of magnesium chloride hexahydrate are added, and the stirring is continued for 1.5 h, and then the mixture is added into a high-pressure reactor, and the temperature of the high-pressure reactor is controlled to 85° C. after the high-pressure reactor is sealed, and the mixture is allowed to stand for 28 h, and then naturally cooled to room temperature to obtain a micellar solution encapsulating magnesium hydroxide;
[0080] 6. Calcination: Calcinate the mixed powder, control the calcination temperature to 520°C, and the calcination time to 4.5 hours to obtain an acid absorbent for EVA film.
[0081] The mass content of magnesium oxide in the acid absorber for EVA film obtained in this embodiment is 89.5%.
[0082] Example 3
[0083] A method for preparing an acid absorbent for EVA film, specifically comprising:
[0084] 1. Light calcination: crush and grind the magnesite to a particle size of 300 mesh, then calcine it at a temperature of 900°C for 2 hours, and then naturally cool it to 250°C to obtain light calcined magnesium oxide powder;
[0085] The mass content of magnesium oxide in the magnesite is 44.7%;
[0086] 2. Hydration: 550 g of light-burned magnesium oxide powder was mixed with 4000 mL of water, stirred at a stirring speed of 100 rpm for 40 min, and then ball milled, with the ball-to-material ratio during ball milling controlled at 5:1, the rotation speed at 400 rpm, and the time at 60 min. Then, heating and stirring were performed, with the temperature during heating and stirring controlled at 120 ° C, the rotation speed at 200 rpm, and the time at 4 h to obtain a hydrated slurry;
[0087] 3. Filtration: Filter the hydrated slurry using a filter screen with a mesh size of 80, remove the filter residue, and obtain the filtered hydrated slurry;
[0088] 4. Primary mixing: 3500 mL of the filtered hydrated slurry was mixed with 15 g of magnesium oxide nanoparticles, stirred at a stirring speed of 200 rpm for 40 min, and then ball milled. The ball-to-material ratio during ball milling was controlled to be 13:1, the rotation speed was 400 rpm, and the time was 60 min to obtain a mixed slurry;
[0089] The preparation method of the magnesium oxide nanoparticles is:
[0090] (1) Preparing a first mixed solution: Mix 35 g of magnesium chloride hexahydrate with 150 mL of water, stir at a stirring speed of 200 rpm for 40 min, add 300 mL of a 4% aqueous solution of the template F127, continue stirring for 40 min, dropwise add 100 mL of a 20% aqueous solution of sodium hydroxide, control the dropping speed to 6 mL / min, and continue stirring for 20 min after the addition is completed to obtain a first mixed solution;
[0091] (2) preparing a second mixed solution: mixing 35 g of magnesium chloride hexahydrate with 150 mL of water, stirring at a stirring speed of 200 rpm for 40 min, adding 400 mL of a 1% sodium dodecylbenzene sulfonate aqueous solution, continuing to stir for 40 min, and dripping 120 mL of a 20% sodium hydroxide aqueous solution at a dripping speed of 6 mL / min. After the dripping is completed, stirring is continued for 20 min to obtain a second mixed solution;
[0092] (3) Hydrothermal treatment: 150 mL of the first mixed solution and 110 mL of the second mixed solution were added to a high-pressure reactor. After the high-pressure reactor was sealed, the temperature of the high-pressure reactor was controlled to 120°C, and the reactor was allowed to stand for 50 hours, and then naturally cooled to room temperature, and then centrifuged at a speed of 10,000 rpm for 15 minutes. After washing the precipitate with water, the precipitate was vacuum dried at 80°C, and then calcined at a temperature of 550°C for 4 hours to obtain magnesium oxide nanoparticles.
[0093] 5. Secondary mixing: 3200 mL of the mixed slurry was dried at a temperature of 140°C for 20 h, then mixed with 150 mL of a micellar solution containing magnesium hydroxide and ball milled at a ball-to-material ratio of 13:1, a rotation speed of 400 rpm, and a time of 4.5 h, and then dried at a temperature of 140°C for 15 h to obtain a mixed powder;
[0094] The preparation method of the micellar solution encapsulating magnesium hydroxide is as follows: 7 mL of concentrated hydrochloric acid with a mass concentration of 36% and 100 mL of anhydrous ethanol are mixed, and the mixture is stirred at 40° C. and 400 rpm for 40 min, and then 3 g of citric acid, 18 g of template F127, and 10 g of magnesium chloride hexahydrate are added, and the stirring is continued for 1.5 h, and then the mixture is added into a high-pressure reactor, and after the high-pressure reactor is sealed, the temperature of the high-pressure reactor is controlled to 90° C., and the mixture is allowed to stand for 30 h, and naturally cooled to room temperature to obtain a micellar solution encapsulating magnesium hydroxide;
[0095] 6. Calcination: Calcinate the mixed powder, control the calcination temperature to 550°C, and the calcination time to 4.5 hours to obtain an acid absorbent for EVA film.
[0096] The mass content of magnesium oxide in the acid absorber for EVA film obtained in this embodiment is 89.1%.
[0097] Comparative Example 1
[0098] This comparative example is a modification of the preparation method of Example 2, the purpose of which is to study the effect of the magnesium oxide nanoparticles added in the first mixing in step 4 of Example 2. The specific modification is that the addition of magnesium oxide nanoparticles in the first mixing in step 4 is omitted, that is, the first mixing in step 4 is changed to:
[0099] 3200 mL of the filtered hydrated slurry was taken for ball milling, and the ball-to-material ratio during ball milling was controlled to be 12:1, the rotation speed was 350 rpm, and the time was 50 min to obtain a mixed slurry.
[0100] The remaining operations are the same as those in Example 2.
[0101] The mass content of magnesium oxide in the acid absorber for EVA film obtained in this comparative example is 90.2%.
[0102] Comparative Example 2
[0103] This comparative example is a modification of the preparation method of Example 2, the purpose of which is to study the effect of the micelle solution encapsulating magnesium hydroxide added in the second mixing in step 5 of Example 2. The specific modification is that the addition of the micelle solution encapsulating magnesium hydroxide in the second mixing in step 5 is omitted, and the drying after ball milling is omitted, that is, the second mixing in step 5 is changed to:
[0104] 3000 mL of the mixed slurry was taken for drying, and the drying temperature was controlled to be 130° C. and the drying time was 18 h to obtain a mixed powder.
[0105] The remaining operations are the same as those in Example 2.
[0106] The mass content of magnesium oxide in the acid absorber for EVA film obtained in this comparative example is 89.8%.
[0107] Comparative Example 3
[0108] This comparative example is a change in the preparation method of comparative example 2, and the purpose is to further study the effect of the micelle solution encapsulating magnesium hydroxide added in the secondary mixing in step 5 of Example 2 on the basis of comparative example 2. The specific change is that in the calcination in step 6, ball milling is performed after the mixed powder is calcined, that is, the calcination in step 6 is changed to:
[0109] The mixed powder was calcined at a temperature of 520° C. for 4.5 h, and then ball-milled at a ball-to-material ratio of 12:1, a rotation speed of 350 rpm, and a time of 4 h to obtain a mixed slurry.
[0110] The remaining operations are the same as those in Comparative Example 2.
[0111] The mass content of magnesium oxide in the acid absorber for EVA film obtained in this comparative example is 89.8%.
[0112] Test Example 1
[0113] The specific surface area, citric acid value (CAA value), and iodine absorption value of the acid absorbent for EVA film of Examples 1-3 and Comparative Examples 1-3 were tested, and the test results are as follows:
[0114] Among them, the specific surface area was tested according to the BET method;
[0115] The citric acid value (CAA value) is tested according to the YB / T 4019-2006 standard;
[0116] The iodine absorption value is tested according to HG / T 3928-2012 standard;
[0117]
[0118] Test Example 2
[0119] The acid absorbents for EVA films of Examples 1-3 and Comparative Examples 1-3 were respectively used in the preparation of EVA films, and the specific preparation methods were as follows:
[0120] Preheating the EVA resin to 80°C, then mixing the preheated EVA resin, EVA film acid absorber, cumene peroxide, triallyl isocyanurate, trimethylolpropane trimethacrylate, vinyl triacetoxysilane, bis(2,2,6,6-tetramethyl-4-piperidinyl) sebacate, and antioxidant 1010 in a mass ratio of 80:2:1:0.5:0.4:2:0.5:0.8, and then passing into an extruder for extrusion, controlling the preheating temperature of the extruder to 110°C, the temperature of the plasticizing zone to 115°C, and the die head temperature to 105°C, and then calendering, cooling and forming, controlling the cooling temperature to 50°C, and then cross-linking, controlling the cross-linking temperature to 150°C, and the time to 50s to obtain an EVA film with a thickness of 0.5 mm;
[0121] The mass content of VA (vinyl acetate) in the EVA resin is 33%;
[0122] Then the average thickness uniformity, light transmittance and bonding strength to glass of the prepared EVA film were tested respectively. The test results are as follows:
[0123] The test method for average thickness uniformity is as follows: take one EVA film sample prepared by the acid absorbent for EVA film of Examples 1-3 and Comparative Examples 1-3, the sample shape is square, the length and width are both 50 cm, measure the thickness at the four vertices and the center point of each EVA film sample, take the maximum thickness and the minimum thickness, and then calculate the thickness uniformity, the calculation formula is as follows:
[0124] Thickness uniformity = (maximum thickness - minimum thickness) / maximum thickness × 100%;
[0125] Then, two more samples were taken, and after testing and calculating the thickness uniformity according to the above method, the average value of the thickness uniformity of each EVA film was calculated respectively;
[0126] The light transmittance is tested according to GB / T 29848-2013 standard;
[0127] The bonding strength of glass is tested according to GB / T 2790-1995 standard;
[0128]
[0129] Further, 10 EVA film samples prepared from the acid absorbents for EVA films of Examples 1-3 and Comparative Examples 1-3 were taken, each of which was square in shape, with a length and a width of 50 cm. The samples were placed in an environment with a temperature of 25° C. and a relative humidity of 80% for 10 days, and the deformation of the EVA film samples was observed. The observation results were as follows:
[0130]
[0131] It can be seen from the results of Experimental Examples 1-2 that by adding magnesium oxide nanoparticles in the preparation of the acid absorber for EVA film, the specific surface area and iodine absorption value of the acid absorber for EVA film can be increased, the citric acid value of the acid absorber for EVA film can be reduced, the problem of easy swelling due to water absorption of the acid absorber for EVA film can be avoided, and the bonding strength of the EVA film prepared by the acid absorber for EVA film to the glass can be improved;
[0132] By adding a micellar solution encapsulating magnesium hydroxide in the preparation of an acid absorber for EVA film, the specific surface area and iodine absorption value of the acid absorber for EVA film can be increased, the citric acid value of the acid absorber for EVA film can be reduced, the light transmittance of the EVA film prepared by the acid absorber for EVA film and the bonding strength to glass can be increased, and the average thickness uniformity of the EVA film prepared by the acid absorber for EVA film can be reduced.
[0133] Unless otherwise specified, all percentages used in the present invention are by mass.
[0134] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an acid absorbent for EVA film, It is characterized in that The method comprises the following steps: light burning, hydration, filtration, primary mixing, secondary mixing, and calcination; The light burning comprises crushing and grinding the magnesite, then calcining and cooling to obtain light burned magnesium oxide powder; The hydration comprises mixing light-burned magnesium oxide powder with water, stirring, and then ball milling and heating and stirring to obtain a hydrated slurry; The primary mixing comprises mixing the filtered hydrated slurry with magnesium oxide nanoparticles, stirring, and then ball milling to obtain a mixed slurry; The method for preparing magnesium oxide nanoparticles comprises the following steps: preparing a first mixed solution, preparing a second mixed solution, and hydrothermally treating; The first mixed solution is prepared by mixing magnesium chloride hexahydrate with water, stirring, adding a template F127 aqueous solution, continuing to stir, and dripping a sodium hydroxide aqueous solution. After the dripping is completed, stirring is continued to obtain a first mixed solution; The second mixed solution is prepared by mixing magnesium chloride hexahydrate with water, stirring, adding an aqueous solution of sodium dodecylbenzenesulfonate, continuing to stir, and dripping an aqueous solution of sodium hydroxide. After the dripping is completed, stirring is continued to obtain a second mixed solution; The hydrothermal treatment comprises adding the first mixed solution and the second mixed solution into a high-pressure reactor, sealing the high-pressure reactor, controlling the temperature of the high-pressure reactor to 110-120° C., standing, naturally cooling to room temperature, and then centrifuging, washing the precipitate, vacuum drying, and then calcining to obtain magnesium oxide nanoparticles; The secondary mixing is to take the mixed slurry and perform primary drying, then mix it with the micelle solution encapsulating magnesium hydroxide, then perform ball milling, and then perform secondary drying to obtain a mixed powder; The preparation method of the micelle solution encapsulating magnesium hydroxide comprises the following steps: mixing concentrated hydrochloric acid and anhydrous ethanol, stirring at 30-40° C., then adding citric acid, template agent F127 and magnesium chloride hexahydrate, continuing stirring, and then adding the mixture into a high-pressure reactor, sealing the high-pressure reactor, controlling the temperature of the high-pressure reactor to 80-90° C., standing, and cooling to obtain the micelle solution encapsulating magnesium hydroxide.
2. The method for preparing the acid scavenger for EVA film according to claim 1, It is characterized in that In the light calcination, the calcination temperature is 800-900° C. and the calcination time is 1.5-2 hours.
3. The preparation method of the acid absorbent for EVA film according to claim 1, It is characterized in that In the hydration, the mass volume ratio of light-burned magnesium oxide powder to water is 500-550g:3500-4000mL; The ball-to-material ratio during the ball milling is 4-5:1, the rotation speed is 350-400rpm, and the time is 40-60min; The temperature during the heating and stirring is 90-120° C., the rotation speed is 100-200 rpm, and the time is 3-4 hours.
4. The method for preparing the acid scavenger for EVA film according to claim 1, It is characterized in that The filtering is to filter the hydrated slurry and remove the filter residue to obtain the filtered hydrated slurry.
5. The preparation method of the acid absorbent for EVA film according to claim 1, It is characterized in that In the primary mixing, the mass volume ratio of the filtered hydrated slurry to the magnesium oxide nanoparticles is 3000-3500 mL:14-15 g; The ball-to-material ratio during the ball milling is 10-13:1, the rotation speed is 350-400 rpm, and the time is 40-60 min.
6. The method for preparing the acid scavenger for EVA film according to claim 1, It is characterized in that In the preparation of the first mixed solution, the mass volume ratio of magnesium chloride hexahydrate, water, template agent F127 aqueous solution, and sodium hydroxide aqueous solution is 32-35g:120-150mL:250-300mL:90-100mL; The mass concentration of the template F127 aqueous solution is 4%; The mass concentration of the sodium hydroxide aqueous solution is 20%; The dropping speed of the sodium hydroxide aqueous solution is 5-6 mL / min; In the preparation of the second mixed solution, the mass volume ratio of magnesium chloride hexahydrate, water, sodium dodecylbenzenesulfonate aqueous solution, and sodium hydroxide aqueous solution is 32-35g:120-150mL:370-400mL:100-120mL; The mass concentration of the sodium dodecylbenzenesulfonate aqueous solution is 1%; The mass concentration of the sodium hydroxide aqueous solution is 20%; The dropping speed of the sodium hydroxide aqueous solution is 5-6 mL / min.
7. The preparation method of the acid absorbent for EVA film according to claim 1, It is characterized in that In the hydrothermal treatment, the volume ratio of the first mixed liquid to the second mixed liquid is 140-150:100-110; The calcination temperature is 500-550°C and the calcination time is 3.5-4h.
8. The method for preparing the acid scavenger for EVA film according to claim 1, It is characterized in that In the secondary mixing, the volume ratio of the mixed slurry to the micelle solution encapsulating magnesium hydroxide is 2900-3200:140-150; The primary drying temperature is 120-140°C and the time is 17-20h; The ball-to-material ratio during the ball milling is 10-13:1, the rotation speed is 350-400 rpm, and the time is 4-4.5 hours; The temperature during the secondary drying is 120-140° C. and the time is 13-15 hours.
9. The method for preparing the acid scavenger for EVA film according to claim 1, It is characterized in that In the preparation of the micellar solution encapsulating magnesium hydroxide, the mass volume ratio of concentrated hydrochloric acid, anhydrous ethanol, citric acid, template F127, and magnesium chloride hexahydrate is 6-7 mL: 90-100 mL: 2.5-3 g: 16-18 g: 9-10 g; The mass concentration of the concentrated hydrochloric acid is 36%.
10. The method for preparing the acid absorbent for EVA film according to claim 1, It is characterized in that The calcining is to calcine the mixed powder to obtain an acid absorbent for EVA film; During the calcination, the calcination temperature is 500-550° C. and the calcination time is 4-4.5 hours.
Citation Information
Patent Citations
Method for preparing magnesium-aluminum hydrotalcite by utilizing magnesite
CN113104871A
Novel acid acceptor and application thereof in polymer system
CN116081679A