A coal-fired catalyst and its preparation method and application
Through coal-fired catalysts with rare earth nitrates, metal oxides and other components, the problems of weak permeability and harmful gas emissions during combustion of block raw coal are solved, and efficient combustion and environmentally friendly emission reduction effects are achieved.
Patent Information
- Application Number
- CN202411009261.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-26
AI Technical Summary
The existing coal-fired catalysts have weak permeability and poor homogenization and dispersion during the combustion of block raw coal, which cannot effectively reduce harmful gas emissions, and there are problems with environmental pollution risks and energy waste.
Coal-fired catalysts using rare earth nitrates, metal oxides, transition metal salts, alkali metal salts and organic acids to form complex salts and metal ions embedded in carbon lattices to reduce coal combustion activation energy and improve permeability and adsorption capacity. and catalytic activity, promote combustion reactions, and reduce SO2 emissions.
It significantly improves the combustion rate and efficiency of coal, reduces harmful gas emissions, reduces coal usage and production costs, and ensures safe and environmentally friendly use of materials.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a coal-fired catalyst and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Coal-fired power generation produces a large amount of waste gas, including SO 2 , CO 2 , CH 4 、N 2 O, etc. Due to outdated combustion equipment, backward combustion technology, and incomplete coal combustion, the thermal efficiency of the equipment is generally low, and energy waste is extremely serious. Therefore, how to improve the thermal efficiency of equipment by improving the coal combustion efficiency to achieve the purpose of energy conservation and emission reduction has become a technical problem that needs to be solved urgently.
[0004] Catalytic combustion-supporting technology can significantly improve the combustion characteristics of raw coal by adding coal-burning catalysts or coal-saving agents to the coal. It can not only increase the volatilization rate of raw coal, reduce the ignition temperature of coal, accelerate the coal burnout rate, reduce ash and carbon residue, and improve combustion efficiency, but also has the secondary effects of desulfurization and denitrification. The existing coal-saving agents still have the following problems in the large-scale application of coal-fired power plant boilers:
[0005] 1. Most coal-saving agents are of the thermal type. They reduce the amount of raw coal used by introducing heat during the boiler calcination process, but do not truly improve the utilization rate of coal resources.
[0006] 2. Most coal-saving agents are made from a mixture of solid and hazardous wastes, posing an environmental pollution risk.
[0007] 3. Most coal-saving agents only reduce coal consumption but do not reduce SO 2 、NO X And other harmful gas emissions.
[0008] 4. The existing coal-saving agents have weak penetration and adsorption capabilities in the combustion application of lump raw coal, poor homogenization and dispersion effects, and their catalytic capabilities cannot be fully exerted or there are problems with boiler calcination fluctuations. Summary of the invention
[0009] The purpose of the present invention is to provide a coal-fired catalyst which has strong permeability and adsorption capacity in lump raw coal, good homogenization and dispersion effect and reduces harmful gas emissions. It also provides a preparation method of the coal-fired catalyst and the application of the coal-fired catalyst in the process of coal-fired power generation using lump raw coal to solve the problems existing in the above-mentioned prior art.
[0010] Specifically, the technical solution of the present invention is as follows:
[0011] In a first aspect of the present invention, a coal-fired catalyst is provided, comprising the following components by mass percentage: 2.5%-6% rare earth nitrate, 0.4%-1.6% metal oxide, 0.5%-1.2% transition metal salt, 3%-12% alkali metal salt, 10%-15% alkaline earth metal salt, 0.2%-1.5% organic acid, and the rest is water, totaling 100%.
[0012] In a specific embodiment, the rare earth nitrate includes one or more of cerium nitrate, lanthanum nitrate, and zirconium nitrate.
[0013] In a specific embodiment, the metal oxide includes one or more of cerium oxide, zinc oxide, and manganese dioxide.
[0014] In a specific embodiment, the transition metal salt includes one or more of copper sulfate, copper nitrate, zinc nitrate, nickel nitrate, zinc chloride, and permanganate.
[0015] In a specific embodiment, the alkali metal salt is a chloride salt, an iodide salt or a nitrate salt of an alkali metal, and the alkali metal is selected from sodium or potassium; preferably, the alkali metal salt includes one or more of sodium chloride, potassium chloride, potassium iodide, potassium nitrate and sodium nitrate.
[0016] In a specific embodiment, the alkaline earth metal salt is a chloride, carbonate or sulfate of an alkaline earth metal, and the alkaline earth metal is selected from barium, magnesium and calcium. Preferably, the alkaline earth metal salt includes one or more of calcium chloride, calcium carbonate, barium carbonate and magnesium sulfate.
[0017] In a specific embodiment, the organic acid includes one or more of citric acid, oxalic acid, tartaric acid, and malic acid.
[0018] In the present invention, alkali metal ions can form complex salts with oxygen-containing groups on the surface of coal, and these complex salts can be connected with aromatic carbon and aliphatic carbon. Due to the electron gain and loss effect of alkali metal elements, oxygen is transferred to the carbon ring or carbon chain to generate CO, CO 2 The water molecules overflow and re-form complex salts, and the surface complex salts play the role of reactive active centers. During the catalytic reaction, the alkali metal oxides produced by the reaction act as oxygen carriers, promoting the diffusion of oxygen in the air to the carbon surface and accelerating the combustion of carbon.
[0019] In the present invention, metal ions are embedded in the carbon lattice to change the microstructure of carbon. Metal ions act as electron donors and promote the speed of some reactions through electron transfer. The metal ions in the catalyst are more active during the heating process, so that their own electrons are transferred to become electron donors, and the metal ions form holes, which causes the electronic structure of the carbon surface to change. The rate of some reactions is accelerated through the transfer of charge, thereby increasing the speed of the entire combustion reaction.
[0020] In the present invention, alkali metal salts, alkaline earth metal salts and metal oxides are used as catalysts, the activation energy of the coal combustion reaction is reduced, and a low-energy consumption reaction pathway is provided for the coal combustion reaction process.
[0021] In the present invention, the rare earth nitrate can react with the organic acid to generate a certain stable ion-associated compound, which has strong hydrophobicity, can improve the interface resistance between the combustion promoter and the coal interface, change the pore structure of the coal, and thus improve the penetration and adsorption capacity of the combustion promoter. At the same time, the rare earth compound can promote the selective oxidation of the NH bond with the Lewis acid, which is beneficial to the metal activity on the catalyst surface and catalyzes the oxidation combustion.
[0022] In the present invention, various chemical components in the coal-fired catalyst quickly penetrate and adsorb into the coal through the coal gaps. When the coal enters the combustion chamber, the various chemical components contained in the coal-fired catalyst act as catalytically active carriers, reduce the ignition point temperature of the coal, reduce the activation energy, and promote the stability of combustion and working conditions. When the product enters the combustion, the flame will be obviously bright and the temperature will rise. As time goes by, the furnace temperature rises, and the steam volume and boiler output will increase. Generally, after the first and second boiler thermal balances, the boiler reaches the optimal state.
[0023] In the present invention, the catalytic action of each component of the coal-fired catalyst promotes SO 2 The reaction with minerals in coal improves the sulfur fixation capacity of coal ash, thereby reducing SO in flue gas. 2 concentration, while improving the ignition performance of coal and accelerating subsequent combustion, reducing SO 2 The existence range increases from about 300℃ to about 500℃, reducing SO during the combustion process 2 The total amount of emissions. The coal is fully burned, the specific surface area of the ash is increased, and harmful gases such as sulfur in the flue gas are adsorbed, while the amount of coal used is reduced, and sulfur emissions and particulate matter emissions are reduced. The coal-fired catalyst provided in this application has the effects of catalytic combustion, sulfur fixation and denitrification, and improving the combustion characteristics of lump raw coal.
[0024] In a second aspect of the present invention, a method for preparing the coal-fired catalyst according to the first aspect is provided, comprising the following steps:
[0025] (1) Add water to a compounding container, and then add rare earth nitrate, alkali metal salt, alkaline earth metal salt, transition metal salt, metal oxide and organic acid in sequence;
[0026] (2) After sufficient stirring, the solid content of the mixture is 18-30wt% and the density is 1.05-1.25g / cm 3 , pH is 0.5-5, and a coal-fired catalyst is obtained.
[0027] Preferably, in step (1), the time interval between the addition of each component is 3-7 minutes, more preferably 5 minutes.
[0028] In a third aspect of the present invention, there is provided a use of the coal-fired catalyst described in the first aspect in a lump raw coal-fired power generation process.
[0029] In a specific embodiment, the application method is: adding the coal-fired catalyst or its dilution into lump raw coal for combustion. Preferably, the amount of the coal-fired catalyst is 0.7-1.2‰ of the weight of the lump raw coal.
[0030] The present invention has the following beneficial effects:
[0031] The coal-fired catalyst of the present invention has stronger penetration and adsorption capacity, solves the problem of uneven dispersion of the catalyst in lump coal, promotes full combustion of coal, increases the coal combustion rate and burnout rate, and improves the application range of the catalyst.
[0032] The raw materials used in the coal-fired catalyst of the present invention do not contain solid hazardous waste and are safe and environmentally friendly.
[0033] The coal-fired catalyst of the present invention not only saves the amount of coal used and reduces the production cost of the enterprise during the combustion process, but also reduces SO 2 、NO X Emission of pollutants. DETAILED DESCRIPTION
[0034] The following examples are only used to illustrate the embodiments of the present invention and do not constitute any limitation to the present invention. Those skilled in the art will appreciate that various modifications may be made without departing from the spirit and scope of the present invention, and these modifications all fall within the scope of protection of the present invention.
[0035] Example 1: A coal-fired catalyst comprising the following components by mass percentage:
[0036] 2.5% cerium nitrate, 0.4% manganese dioxide, 0.5% nickel nitrate, 3% sodium nitrate, 10% barium carbonate, 0.2% malic acid, and the rest is water.
[0037] The preparation method of the coal-fired catalyst is as follows:
[0038] (1) Add water to a compounding container, and then add cerium nitrate, sodium nitrate, barium carbonate, nickel nitrate, manganese dioxide and malic acid in sequence while stirring; the time interval between adding each raw material component is 5 minutes.
[0039] (2) After sufficient stirring, the solid content of the mixture was controlled at 18 wt% and the density was controlled at 1.05 g / cm 3 , the coal-fired catalyst was obtained at pH 0.5.
[0040] Embodiment 2: The rest is the same as Embodiment 1, except that:
[0041] The coal-fired catalyst includes the following components by mass percentage: 4% zirconium nitrate, 0.8% zinc oxide, 0.8% copper permanganate, 5% potassium iodide, 12% calcium carbonate, 0.5% malic acid, and the rest is water.
[0042] The time interval between adding each raw material component is 3 minutes.
[0043] The solid content of the mixture was controlled at 24wt% and the density was controlled at 1.15g / cm 3 , pH at 3.0.
[0044] Embodiment 3: The rest is the same as Embodiment 1, except that:
[0045] The coal-fired catalyst includes the following components by mass percentage: 5% lanthanum nitrate, 1.2% manganese dioxide, 1.0% copper sulfate, 8% potassium nitrate, 14% magnesium sulfate, 1.0% malic acid, and the rest is water.
[0046] The time interval between adding each raw material component is 7 minutes.
[0047] The solid content of the mixture is controlled at 30wt% and the density is controlled at 1.25g / cm 3 , pH at 5.0.
[0048] Embodiment 4: The rest is the same as Embodiment 1, except that:
[0049] The coal-fired catalyst includes the following components by mass percentage: 6% zirconium nitrate, 1.6% zinc oxide, 1.2% zinc nitrate, 12% potassium iodide, 15% calcium carbonate, 1.5% malic acid, and the rest is water.
[0050] The solid content of the mixture was controlled at 22wt% and the density was controlled at 1.18g / cm 3 , pH at 2.5.
[0051] Comparative Example 1: The rest is the same as Example 1, except that:
[0052] The cerium nitrate was replaced by samarium nitrate.
[0053] Comparative Example 2: The rest is the same as Example 1, except that:
[0054] The cerium nitrate was replaced by praseodymium nitrate.
[0055] Comparative Example 3: The rest is the same as Example 1, except that:
[0056] Nickel nitrate was replaced by aluminum silicate.
[0057] Comparative Example 4: The rest is the same as Example 1, except that:
[0058] Nickel nitrate was replaced by zinc hydroxide.
[0059] Comparative Example 5: The rest is the same as Example 1, except that:
[0060] Barium carbonate was replaced by calcium oxalate.
[0061] Comparative Example 6: The rest is the same as Example 1, except that:
[0062] The barium carbonate was replaced with calcium ammonium nitrate.
[0063] Comparative Example 7: The rest is the same as Example 1, except that:
[0064] Manganese dioxide was replaced by nickel oxide.
[0065] Comparative Example 8: The rest is the same as Example 1, except that:
[0066] Manganese dioxide was replaced by manganese nitrate.
[0067] Comparative Example 9: The rest is the same as Example 1, except that:
[0068] Sodium nitrate was replaced by sodium bromide.
[0069] Comparative Example 10: The rest is the same as Example 1, except that:
[0070] Sodium nitrate was replaced with potassium bromide.
[0071] Comparative Example 11: The rest is the same as Example 1, except that:
[0072] Malic acid and cerium nitrate were replaced with an equal amount of water.
[0073] The coal-fired catalyst samples prepared in Examples 1-4 and Comparative Examples 1-11 were uniformly mixed with the same weight of lump coal at a weight ratio of 1‰, and then subjected to combustion and power generation tests. After 20 minutes of combustion, samples were taken to test the porosity of the coal and to detect the SO generated by the combustion. 2The results of gas volume are shown in Table 1 below.
[0074] Table 1 Effects of different coal-fired catalysts on the combustion of lump coal
[0075] Group Porosity of coal (%) <![CDATA[SO 2 Production volume (L / kg)]]> Coal consumption for power generation (g / kwh) Example 1 26.9 0.51 281 Example 2 27.0 0.52 283 Example 3 27.1 0.52 282 Example 4 26.8 0.51 281 Comparative Example 1 22.3 0.67 290 Comparative Example 2 21.9 0.71 291 Comparative Example 3 22.6 0.68 289 Comparative Example 4 21.4 0.72 292 Comparative Example 5 21.8 0.68 291 Comparative Example 6 22.4 0.69 292 Comparative Example 7 22.3 0.66 291 Comparative Example 8 21.2 0.67 290 Comparative Example 9 20.9 0.69 291 Comparative Example 10 21.6 0.70 292 Comparative Example 11 22.9 0.73 293
[0076] The results in Table 1 show that the coal porosity of Comparative Example 11 is significantly lower than that of Example 1, indicating that the combination of rare earth nitrate and organic acid can effectively improve the porosity of bulk raw coal, optimize the pore structure, promote the rapid penetration of each component in the catalyst into the interior of the bulk raw coal, and play a role in promoting combustion. Therefore, the coal consumption for power generation in Example 1 is also significantly lower than that in Comparative Example 11. The coal porosity of Comparative Examples 1 and 2 is also significantly lower than that in Example 1, indicating that the type and combination of rare earth nitrate and organic acid are crucial to the improvement of the penetration effect of the catalyst. Only a few specific types of rare earth nitrate and organic acid can achieve efficient penetration enhancement effect. The coal porosity of Comparative Examples 3-10 is significantly lower than that of Example 1, and the coal consumption for power generation is significantly higher than that of Example 1, indicating that the penetration enhancement effect produced by the combination of malic acid and cerium nitrate also depends on the catalytic support system formed by the other components. When the components in the catalytic support system are changed, malic acid and cerium nitrate cannot play a penetration enhancement role, which directly leads to the loss of the coal-saving effect of the catalyst. The various components in the coal-fired catalyst of the present invention cooperate with each other to jointly enhance the penetration enhancement effect and the combustion promotion effect, thereby reducing the emission of sulfur dioxide and lowering the coal consumption for power generation.
[0077] The coal-fired catalyst of the present invention has achieved good coal-saving and emission reduction effects when used in multiple coal-fired power plants. For example: (1) The amount of the coal-fired catalyst is 0.7‰ of the weight of the lump raw coal. When it is used in the 32#300MW unit of a power plant in Sichuan, the coal consumption for power generation is reduced by 7.39g / kwh. (2) The amount of the coal-fired catalyst is 1.2‰ of the weight of the lump raw coal. When it is used in the 1#350MW unit of a power plant in Henan, the coal consumption for power generation is reduced by 5.23g / kwh.
[0078] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A coal-fired catalyst, characterized in that: In terms of mass percentage, it includes the following components: Rare earth nitrate 2.5%-6%, metal oxide 0.4%-1.6%, transition metal salt 0.5%-1.2%, alkali metal salt 3%-12%, alkaline earth metal salt 10%-15%, organic acid 0.2%-1.5%, the rest is water, totaling 100%; The organic acid is malic acid; The rare earth nitrate is one or more of cerium nitrate, lanthanum nitrate and zirconium nitrate; The metal oxide is one or more of zinc oxide and manganese dioxide; The transition metal salt is one or more of sulfates, nitrates, and permanganates of transition metals, and the transition metal is one or more of copper, zinc, and nickel; The alkali metal salt is one or more of iodine salt and nitrate; The alkaline earth metal salt is a carbonate of an alkaline earth metal, and the alkaline earth metal is barium.
2. A method for preparing the coal-fired catalyst according to claim 1, comprising the following steps: (1) Add water to a compounding container, and then add rare earth nitrate, alkali metal salt, alkaline earth metal salt, transition metal salt, metal oxide and organic acid in sequence; (2) After sufficient stirring, the solid content of the mixture is 18-30wt% and the density is 1.05-1.25g / cm 3 , the coal-fired catalyst is obtained at a pH of 0.5-5.
3. The method for preparing the coal-fired catalyst according to claim 2, characterized in that: In step (1), the time interval between the addition of each component is 3-7 minutes.
4. Use of the coal-fired catalyst according to claim 1 in a coal-fired power generation process using lump raw coal.
5. The use according to claim 4, characterized in that: The application method is: adding the coal-fired catalyst or the diluted solution of the coal-fired catalyst into lump raw coal for combustion, and the amount of the coal-fired catalyst used is 0.7-1.2‰ of the weight of the lump raw coal.