Ultrafine tungsten oxide particles and preparation method and application thereof, catalytic oxidation catalyst and preparation method and application thereof

The systolic oxide particles with narrow particle size distribution and high specific surface area were synthesized by the solvent-thermal reaction method. As a catalyst support, the problems of poor stability and high cost in the preparation of existing tungsten oxide materials were solved, the catalytic performance was improved, and the reaction temperature was reduced, thus achieving the goal of Efficient CO catalytic oxidation.

CN118529778BActive Publication Date: 2024-11-15江西中科鸿虔新材料有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411008325.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-15
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

Among the existing preparation methods for tungsten oxide materials, the sol-gel method has poor stability, high cost of chemical vapor deposition, and it is difficult to obtain ultrafine tungsten oxide particles with narrow particle size distribution and high specific surface area, which affects its performance in catalytic applications. .

Method used

Using the solvothermal reaction method, tungsten oxide particles were synthesized under mild conditions using template guide agent and dispersion additive and soluble tungsten salt. Tungsten oxide particles with narrow particle size distribution were obtained by drying and calcining, and used as a catalyst support to support the active group. to improve catalytic performance.

Benefits of technology

The narrow particle size distribution and high specific surface area of ​​tungsten oxide particles are achieved, the amount of active components is reduced, the temperature of CO catalytic oxidation reaction is significantly reduced, and the catalytic activity and energy efficiency are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118529778B_ABST
    Figure CN118529778B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of tungsten oxide materials, and in particular to ultrafine tungsten oxide particles, a preparation method and application thereof, a catalytic oxidation catalyst, a preparation method and application thereof; the particle size distribution width of the tungsten oxide particles is 0.1-3.0; the particle size distribution width is calculated as (D 90 ‑D 10 ) / 2D 50 The particle size distribution of the tungsten oxide particles of the present invention is narrow; the tungsten oxide particles of the present invention are used as catalytic oxidation catalyst carriers, which can reduce the amount of active components (such as precious metals) while maintaining catalytic performance; the catalyst of the present invention is used for CO catalytic oxidation, has high catalytic activity, and can significantly reduce the reaction temperature and save energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of tungsten oxide materials, and in particular to ultrafine tungsten oxide particles, a preparation method and application thereof, and a catalytic oxidation catalyst, a preparation method and application thereof. Background Art

[0002] Tungsten oxide is a widely used transition metal oxide with a large number of polymorphs and substoichiometric compositions, with innate tunneling and oxygen vacancies. The structure-determined properties, such as altered light absorption and metal-like conductivity, make tungsten oxide an important material for optoelectronic applications, including not only the traditional electrochromic / photochromic fields, but also visible light-driven photocatalysis, photothermal therapy, etc.

[0003] So far, researchers have used a variety of physical and chemical synthesis methods to prepare tungsten oxide, such as chemical vapor deposition, sol-gel, and hydrothermal methods. The sol-gel method is simple to operate, but the stability of the prepared sol is poor. Chemical vapor deposition products have high purity and are easier to control, but the cost is high. Summary of the invention

[0004] The purpose of the present invention is to provide ultrafine tungsten oxide particles and a preparation method and application thereof, a catalytic oxidation catalyst and a preparation method and application thereof; the tungsten oxide particles of the present invention have a narrow particle size distribution, and the preparation method of the tungsten oxide particles is simple, the conditions are mild, and the repeatability is good.

[0005] In order to achieve the above-mentioned object, the first aspect of the present invention provides an ultrafine tungsten oxide particle, wherein the particle size distribution width of the tungsten oxide particle is 0.1-3.0;

[0006] The particle size distribution width is calculated as (D 90 -D 10 ) / 2D 50 .

[0007] A second aspect of the present invention provides a method for preparing the tungsten oxide particles of the present invention, the method comprising:

[0008] 1) subjecting a solution containing a template directing agent, a soluble tungsten salt, and a dispersing aid to a solvothermal reaction;

[0009] 2) separating the product obtained in step 1) to obtain a solid, drying and calcining to obtain tungsten oxide particles;

[0010] The template directing agent is selected from one or more of oxalic acid, lactic acid, sulfuric acid, citric acid, ammonium acetate and ammonium bicarbonate;

[0011] The dispersing aid is selected from hydrophilic polymers;

[0012] The mass of the soluble tungsten salt is calculated as tungsten oxide, the mass ratio of the template directing agent to the soluble tungsten salt is 0.5-5:1, and the mass ratio of the dispersing aid to the soluble tungsten salt is 0.2-2:1.

[0013] A third aspect of the present invention provides a use of the tungsten oxide particles of the present invention as a catalyst carrier.

[0014] A fourth aspect of the present invention provides a catalytic oxidation catalyst, which includes a carrier and an active component supported on the carrier, wherein the carrier includes the tungsten oxide particles described in the present invention.

[0015] A fifth aspect of the present invention provides a method for preparing a catalytic oxidation catalyst, the method comprising:

[0016] (1) preparing a carrier according to the method for preparing tungsten oxide particles of the present invention;

[0017] (2) The solution containing the active ingredient source is brought into contact with the carrier, the solvent is removed, and the solution is reduced.

[0018] A sixth aspect of the present invention provides an application of the catalytic oxidation catalyst of the present invention or a catalyst prepared by the preparation method of the catalytic oxidation catalyst of the present invention in catalytic oxidation of CO.

[0019] Through the above technical solution, the technical solution of the present invention has the following advantages:

[0020] (1) The tungsten oxide particles of the present invention have a narrow particle size distribution and also have the advantage of a high specific surface area.

[0021] (2) The preparation method of the tungsten oxide particles of the present invention is simple, the conditions are mild, and the repeatability is good.

[0022] (3) The tungsten oxide particles of the present invention are used as catalytic oxidation catalyst carriers, which can reduce the amount of active components (such as precious metals) while maintaining catalytic performance; the catalyst of the present invention is used for CO catalytic oxidation, has high catalytic activity, and can significantly reduce the reaction temperature and save energy. For example, under the implementation conditions of the present invention, T90 (the temperature corresponding to 90% CO conversion rate) is lower than 180°C, and T50 (the temperature corresponding to 50% CO conversion rate) is lower than 165°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Example 1;

[0024] Figure 2 This is a scanning electron microscope (SEM) image of tungsten oxide particles prepared in Example 2;

[0025] Figure 3This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Example 3;

[0026] Figure 4 This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Example 4;

[0027] Figure 5 A scanning electron microscope (SEM) image of tungsten oxide prepared in Comparative Example 1;

[0028] Figure 6 This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Comparative Example 3;

[0029] Figure 7 This is the relationship between CO oxidation conversion rate and temperature in Example 8;

[0030] Figure 8 This is the relationship between CO oxidation conversion rate and temperature in Example 9;

[0031] Fig. 9 This is the relationship between CO oxidation conversion rate and temperature in Example 10;

[0032] Fig.10 This is the relationship between CO oxidation conversion rate and temperature in Example 11;

[0033] Fig.11 This is the relationship between CO oxidation conversion rate and temperature in Example 12;

[0034] Fig.12 This is the relationship between CO oxidation conversion rate and temperature in Example 13;

[0035] Fig.13 The relationship between CO oxidation conversion rate and temperature in Comparative Example 2;

[0036] Fig.14 This is the relationship between CO oxidation conversion rate and temperature in Comparative Example 6. DETAILED DESCRIPTION

[0037] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0038] In the context of this specification, including in the following examples and comparative examples, D 90 , D 10 , D 50They are the measured size values ​​of 90%, 10% and 50% of the particle sizes in the particle size distribution test, respectively. The particle size distribution test is measured by Malvern Mastersizer 3000 laser particle size analyzer.

[0039] In the context of this specification, including in the following examples and comparative examples, the specific surface area test was carried out on a Micromeritics instrument ASAP 2460 and calculated using the BET method ( ), the specific surface area was measured by N2 adsorption; before the N2 adsorption test, the sample was degassed at 300℃ for 6h.

[0040] The first aspect of the present invention provides an ultrafine tungsten oxide particle, wherein the particle size distribution width of the tungsten oxide particle is 0.1-3.0;

[0041] The particle size distribution width is calculated as (D 90 -D 10 ) / 2D 50 The tungsten oxide particles of the present invention have a narrow particle size distribution.

[0042] According to a preferred embodiment of the present invention, the particle size distribution width of the tungsten oxide particles is 1.0-3.0.

[0043] According to a preferred embodiment of the present invention, the specific surface area of ​​the tungsten oxide particles is 1-100 m 2 / g, preferably 1-10m 2 / g.

[0044] According to a preferred embodiment of the present invention, the tungsten oxide particles D 90 The value is 1-100μm, for example, it can be 1.5μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm; preferably it is 1.5-60μm.

[0045] According to a preferred embodiment of the present invention, the tungsten oxide particles D 50 The value is 0.5-30μm, for example, it can be 1μm, 1.5μm, 2μm, 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 12μm, 15μm, 18μm, 20μm, 22μm, 25μm, 28μm; preferably it can be 0.6-22μm.

[0046] According to a preferred embodiment of the present invention, the tungsten oxide particles D 10The value is 0.05-4μm, for example, it can be 0.06μm, 0.08μm, 0.1μm, 0.2μm, 0.5μm, 0.8μm, 1μm, 1.5μm, 2μm, 3μm, 3.5μm, and is preferably 0.1-3μm.

[0047] A second aspect of the present invention provides a method for preparing the tungsten oxide particles of the present invention, the method comprising:

[0048] 1) subjecting a solution containing a template directing agent, a soluble tungsten salt, and a dispersing aid to a solvothermal reaction;

[0049] 2) separating the product obtained in step 1) to obtain a solid, drying and calcining the solid to obtain tungsten oxide particles;

[0050] The template directing agent is selected from one or more of oxalic acid, lactic acid, sulfuric acid, citric acid, ammonium acetate and ammonium bicarbonate;

[0051] The dispersing aid is selected from hydrophilic polymers;

[0052] The mass of the soluble tungsten salt is calculated as tungsten oxide, the mass ratio of the template directing agent to the soluble tungsten salt is 0.5-5:1, and the mass ratio of the dispersing aid to the soluble tungsten salt is 0.2-2:1.

[0053] The preparation method of the tungsten oxide particles of the present invention is simple, has mild conditions and good repeatability. The tungsten oxide particles of the present invention are prepared by performing a solvothermal reaction on a soluble tungsten salt solution containing the template directing agent and the dispersing aid of the present invention.

[0054] In the present invention, the hydrophilic polymer refers to a polymer containing polar or charged functional groups and capable of being dissolved in water.

[0055] According to a preferred embodiment of the present invention, the hydrophilic polymer is selected from one or more of polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA) and polyethylene glycol (PEG). Preferably, the weight average molecular weight of the hydrophilic polymer is 40-130000 g / mol, which is conducive to making the particle size distribution of the tungsten oxide particles narrower.

[0056] In the present invention, the concentration of the soluble tungsten salt in the solution can be selected in a wide range. According to a preferred embodiment of the present invention, the mass of the soluble tungsten salt is calculated as tungsten oxide, and the concentration of the soluble tungsten salt in the solution is 5-50g / L; this is conducive to making the particle size distribution of the tungsten oxide particles narrower.

[0057] In the present invention, in the solution, the types of solvents can be selected from a wide range. According to a preferred embodiment of the present invention, the solvent is selected from water and / or ethanol.

[0058] According to a preferred embodiment of the present invention, the solvent thermal reaction conditions include: a temperature of 150-220°C, preferably 180-220°C; the solvent thermal reaction time can be selected in a wide range, preferably, the reaction time is 8-36h, more preferably 12-36h.

[0059] In the present invention, there is no particular limitation on the calcination conditions, and conventional calcination conditions in the art can achieve the purpose of the present invention.

[0060] This is an exemplary description, but the scope of the present invention is not limited thereto. According to one embodiment of the present invention, the calcination conditions include: a calcination temperature of 500-850°C, preferably 650-750°C, preferably, a calcination time of 1-10h, preferably a calcination time of 1-2h. In the implementation of the present invention, calcination at 700°C for 1h is used as an exemplary description, but the scope of the present invention is not limited thereto.

[0061] According to a preferred embodiment of the present invention, the mass ratio of the template directing agent to the dispersing aid is 1:0.2-1; the catalytic oxidation catalyst prepared by using the tungsten oxide particles prepared under the above conditions can improve the catalytic performance.

[0062] In the present invention, there is no particular limitation on the separation method of the product after the solvothermal reaction, as long as the solid and liquid are separated, for example, the solid and liquid can be separated by filtration, centrifugation, etc.

[0063] In the present invention, impurities on the surface of solid particles are removed by washing. Washing is a conventional operation in the art and is not particularly limited in the present invention.

[0064] In the present invention, there is no particular limitation on the drying conditions of the separated solid, as long as the solvent on the surface of the solid is removed. For example, the solid can be dried at 50-120°C.

[0065] A third aspect of the present invention provides a use of the tungsten oxide particles of the present invention as a catalyst carrier.

[0066] A fourth aspect of the present invention provides a catalytic oxidation catalyst, which includes a carrier and an active component supported on the carrier, wherein the carrier includes the tungsten oxide particles described in the present invention.

[0067] According to a preferred embodiment of the present invention, the content of active components is 0.5-2.5 wt % based on the total mass of the catalyst.

[0068] According to a preferred embodiment of the present invention, based on the total mass of the catalyst, the carrier content is 97.5-99.5wt%.

[0069] In the present invention, the range of element types of the active component is relatively wide, and all active components used for catalysis can be used in the present invention. For example, the active component is selected from one or more of Ru, Rh, Pd and Pt. According to a preferred embodiment of the present invention, the active component is selected from one or more of precious metals, preferably Pt and / or Pd.

[0070] A fifth aspect of the present invention provides a method for preparing a catalytic oxidation catalyst, the method comprising:

[0071] (1) preparing a carrier according to the method for preparing tungsten oxide particles of the present invention;

[0072] (2) The solution containing the active ingredient source is brought into contact with the carrier, the solvent is removed, and the solution is reduced.

[0073] In the present invention, as long as the active component source is loaded on the carrier, there is no particular limitation on the contact conditions.

[0074] In the present invention, the concentration of the solution containing the active component source can be selected in a wide range. According to a preferred embodiment of the present invention, the concentration of the solution containing the active component source is 0.01-0.5 mol / L.

[0075] In the present invention, there is no particular limitation on the method of removing the solvent, as long as the carrier loaded with the active component source can be removed. For example, the solvent can be removed by drying. Preferably, the drying conditions include: a drying temperature of 80-100° C. and a drying time of 8-12 h.

[0076] In the present invention, the active component source is reduced to a single substance by reduction, and the reduction conditions can be selected in a wide range. According to a preferred embodiment of the present invention, the reduction conditions include: a reduction temperature of 200-450°C, a reduction time of 1-24h, preferably 2-4h.

[0077] In the present invention, the reduction is carried out in a reducing gas atmosphere. There is no particular limitation on the type and amount of the reducing gas. For example, the reduction can be carried out in a hydrogen-containing atmosphere, preferably in a hydrogen atmosphere.

[0078] In the present invention, the types of active component sources can be selected from a wide range. According to a preferred embodiment of the present invention, the active component source is selected from one or more soluble salts of active component elements, preferably chloroplatinic acid.

[0079] According to a preferred embodiment of the present invention, the amount of active component source used is such that the active component content is 0.5-2.5 wt % based on the total mass of the catalyst.

[0080] According to a preferred embodiment of the present invention, the amount of the carrier used is such that the carrier content is 97.5-99.5 wt % based on the total mass of the catalyst.

[0081] The sixth aspect of the present invention provides an application of the catalytic oxidation catalyst of the present invention or the catalyst prepared by the preparation method of the catalytic oxidation catalyst of the present invention in the catalytic oxidation of CO. The catalytic oxidation catalyst of the present invention is used for the catalytic oxidation of CO, has high catalytic activity, can significantly reduce the reaction temperature, and saves energy.

[0082] According to a preferred embodiment of the present invention, the application comprises: catalytically oxidizing a raw gas containing CO and O2 in the presence of a catalyst.

[0083] In the present invention, there is no particular limitation on the volume space velocity of the feed gas, and the purpose of the present invention can be achieved under any conventional conditions in the art.

[0084] For exemplary purposes only, but not to limit the scope of the present invention, according to one embodiment of the present invention, the volumetric space velocity of the feed gas is 5000-50000 ml·g cat -1 ·h -1 In the practice of the present invention, 10000 ml·g cat -1 ·h -1 This is intended to be an illustrative example, but does not limit the scope of the invention.

[0085] In the present invention, there is no particular limitation on the catalytic oxidation conditions, and any conventional catalytic oxidation conditions in the art can achieve the purpose of the present invention. For exemplary purposes, but not limiting the scope of the present invention, according to one embodiment of the present invention, the catalytic oxidation conditions include: an oxidation temperature of 130-400°C.

[0086] In the present invention, the volume ratio of CO to O2 can be selected in a wide range. According to a preferred embodiment of the present invention, the volume ratio of CO to O2 is 1:0.5-30. In the implementation of the present invention, the volume ratio of CO to O2 = 1:21 is used as an exemplary illustration, but the scope of the present invention is not limited thereby.

[0087] In the present invention, the raw material gas may further contain an inert gas, such as nitrogen.

[0088] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.

[0089] In the following examples, ammonium metatungstate is used as a soluble tungsten salt by way of example. 2 g of ammonium metatungstate is taken and calcined at 1000° C. for 1 h to obtain 1.74 g of tungsten oxide, thereby determining the tungsten oxide content in the ammonium metatungstate, which is 87%.

[0090] In the following examples, the molecular weights of polyvinyl pyrrolidone (PVP), polyvinyl alcohol (PVA) and polyethylene glycol (PEG) refer to weight average molecular weights.

[0091] Example 1

[0092] 1) Ammonium metatungstate is calculated as tungsten oxide, with a tungsten oxide concentration of 40 g / L, anhydrous oxalic acid concentration of 30 g / L, and a PVP concentration of 20 g / L with a molecular weight of 1,300,000 g / mol. Dissolve ammonium metatungstate, anhydrous oxalic acid, and PVP in deionized water to obtain 1 L of a mixed solution, put the mixed solution into a reactor with a polytetrafluoroethylene liner, and then put the reactor into an oven at 180°C for reaction for 18 hours;

[0093] 2) After the reaction is completed, the reactor is taken out and cooled to room temperature. The cooled solution is taken out and centrifuged for 10 minutes. The precipitate is washed with deionized water and repeated 5 times. The obtained solid is placed in an oven at 80°C and dried for 12 hours, and then calcined at 700°C for 1 hour to obtain tungsten oxide particles.

[0094] Figure 1 This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Example 1, indicating that the tungsten oxide particles were successfully prepared.

[0095] The specific surface area, D 90 , D 10 , D 50 The specific surface area, D 90 , D 10 and D 50 , the test results are shown in Table 1.

[0096] 3) The oxidation catalyst was prepared by loading platinum with the incipient wetness impregnation method. The specific steps included: adding 1.573 g of tungsten oxide to 2 ml of 0.04 mol / L chloroplatinic acid solution and stirring for 1 h, standing for 12 h, and drying at 110°C, and treating at 300°C for 3 h in a 30 ml / min H2 atmosphere.

[0097] Example 2

[0098] 1) Ammonium metatungstate is calculated as tungsten oxide, and the concentration of tungsten oxide is 10g / L, the concentration of lactic acid is 40g / L, and the concentration of PVA with a molecular weight of 44.05g / mol is 20g / L. Dissolve ammonium metatungstate, lactic acid, and PVA in deionized water to obtain 1L of mixed solution, put the mixed solution into a reactor with a polytetrafluoroethylene liner, and then put the reactor into an oven at 180°C for reaction for 18 hours;

[0099] 2) After the reaction is completed, the reactor is taken out and cooled to room temperature. The cooled solution is taken out and centrifuged for 10 minutes. The precipitate is washed with deionized water and repeated 5 times. The obtained solid is placed in an oven at 80°C and dried for 12 hours, and then calcined at 700°C for 1 hour to obtain tungsten oxide particles.

[0100] Figure 2 This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Example 2, indicating that the tungsten oxide particles were successfully prepared.

[0101] The specific surface area, D 90 , D 10 , D 50 The specific surface area, D 90 , D 10 and D 50 , the test results are shown in Table 1.

[0102] 3) The oxidation catalyst was prepared by loading platinum with the incipient wetness impregnation method. The specific steps included: adding 1.573 g of tungsten oxide to 2 ml of 0.04 mol / L chloroplatinic acid solution and stirring for 1 h, standing for 12 h, and drying at 110°C, and treating at 300°C for 3 h in a 30 ml / min H2 atmosphere.

[0103] Example 3

[0104] 1) Ammonium metatungstate is calculated as tungsten oxide, with a tungsten oxide concentration of 30 g / L, a sulfuric acid concentration of 60 g / L, and a PVP concentration of 20 g / L with a molecular weight of 1,300,000 g / mol. Dissolve ammonium metatungstate, sulfuric acid, and PVP in deionized water to obtain 1 L of a mixed solution, place the mixed solution in a reactor with a polytetrafluoroethylene liner, and then place the reactor in an oven at 180°C for reaction for 18 hours;

[0105] 2) After the reaction is completed, the reactor is taken out and cooled to room temperature. The cooled solution is taken out and centrifuged for 10 minutes. The precipitate is washed with deionized water and repeated 5 times. The obtained solid is placed in an oven at 80°C and dried for 12 hours, and then calcined at 700°C for 1 hour to obtain tungsten oxide particles.

[0106] Figure 3 This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Example 3, indicating that the tungsten oxide particles were successfully prepared.

[0107] The specific surface area, D 90 , D 10 , D 50 The specific surface area, D 90 , D 10 and D 50 , the test results are shown in Table 1.

[0108] 3) The oxidation catalyst was prepared by loading platinum with the incipient wetness impregnation method. The specific steps included: adding 1.573 g of tungsten oxide to 2 ml of 0.04 mol / L chloroplatinic acid solution and stirring for 1 h, standing for 12 h, and drying at 110°C, and treating at 300°C for 3 h in a 30 ml / min H2 atmosphere.

[0109] Example 4

[0110] 1) Ammonium metatungstate is calculated as tungsten oxide, with a tungsten oxide concentration of 40 g / L, an ammonium acetate concentration of 70 g / L, and a PVA concentration of 20 g / L with a molecular weight of 44.05 g / mol. Dissolve ammonium metatungstate, ammonium acetate, and PVA in deionized water to obtain 1 L of a mixed solution, put the mixed solution into a reactor with a polytetrafluoroethylene liner, and then put the reactor into an oven at 180°C for reaction for 18 hours;

[0111] 2) After the reaction is completed, the reactor is taken out and cooled to room temperature. The cooled solution is taken out and centrifuged for 10 minutes. The precipitate is washed with deionized water and repeated 5 times. The obtained solid is placed in an oven at 80°C and dried for 12 hours, and then calcined at 700°C for 1 hour to obtain tungsten oxide particles.

[0112] Figure 4 This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Example 4, indicating that the tungsten oxide particles were successfully prepared.

[0113] The specific surface area, D 90 , D 10 , D 50 The specific surface area, D 90 , D 10 and D 50 , the test results are shown in Table 1.

[0114] 3) The oxidation catalyst was prepared by loading platinum with the incipient wetness impregnation method. The specific steps included: adding 1.573 g of tungsten oxide to 2 ml of 0.04 mol / L chloroplatinic acid solution and stirring for 1 h, standing for 12 h, and drying at 110°C, and treating at 300°C for 3 h in a 30 ml / min H2 atmosphere.

[0115] Example 5

[0116] 1) Ammonium metatungstate is calculated as tungsten oxide, with a tungsten oxide concentration of 40 g / L, anhydrous oxalic acid concentration of 60 g / L, and a PVP concentration of 10 g / L with a molecular weight of 1,300,000 g / mol. Dissolve ammonium metatungstate, anhydrous oxalic acid, and PVP in deionized water to obtain 1 L of a mixed solution, put the mixed solution into a reactor with a polytetrafluoroethylene liner, and then put the reactor into an oven at 180°C for reaction for 18 hours;

[0117] 2) After the reaction is completed, the reactor is taken out and cooled to room temperature. The cooled solution is taken out and centrifuged for 10 minutes. The precipitate is washed with deionized water and repeated 5 times. The obtained solid is placed in an oven at 80°C and dried for 12 hours, and then calcined at 700°C for 1 hour to obtain tungsten oxide particles.

[0118] The specific surface area, D 90 , D 10 , D 50 The specific surface area, D 90 , D 10 and D 50 , the test results are shown in Table 1.

[0119] 3) The oxidation catalyst was prepared by loading platinum with the incipient wetness impregnation method. The specific steps included: adding 1.573 g of tungsten oxide to 2 ml of 0.04 mol / L chloroplatinic acid solution and stirring for 1 h, standing for 12 h, and drying at 110°C, and treating at 300°C for 3 h in a 30 ml / min H2 atmosphere.

[0120] Example 6

[0121] 1) Based on tungsten oxide, the concentration of ammonium metatungstate is 40g / L, the concentration of anhydrous oxalic acid is 20g / L, and the concentration of PVP with a molecular weight of 1300000g / mol is 10g / L. Dissolve ammonium metatungstate, anhydrous oxalic acid, and PVP in deionized water to obtain 1L of mixed solution. Put the mixed solution into a reactor with a polytetrafluoroethylene liner, and then put the reactor into an oven at 180°C for reaction for 18 hours;

[0122] 2) After the reaction is completed, the reactor is taken out and cooled to room temperature. The cooled solution is taken out and centrifuged for 10 minutes. The precipitate is washed with deionized water and repeated 5 times. The obtained solid is placed in an oven at 80°C and dried for 12 hours, and then calcined at 700°C for 1 hour to obtain tungsten oxide particles.

[0123] The specific surface area, D 90 , D 10 , D 50 The specific surface area, D 90 , D 10 and D 50, the test results are shown in Table 1.

[0124] 3) The oxidation catalyst was prepared by loading platinum with the incipient wetness impregnation method. The specific steps included: adding 1.573 g of tungsten oxide to 2 ml of 0.04 mol / L chloroplatinic acid solution and stirring for 1 h, standing for 12 h, and drying at 110°C, and treating at 300°C for 3 h in a 30 ml / min H2 atmosphere.

[0125] Example 7

[0126] 1) Ammonium metatungstate is calculated as tungsten oxide, with a tungsten oxide concentration of 50 g / L, a citric acid concentration of 25 g / L, and a polyethylene glycol concentration of 25 g / L with a molecular weight of 400 g / mol. Dissolve ammonium metatungstate, citric acid, and polyethylene glycol in deionized water to obtain 1 L of a mixed solution, put the mixed solution into a reactor with a polytetrafluoroethylene liner, and then put the reactor into an oven at 220°C for reaction for 12 hours;

[0127] 2) After the reaction is completed, the reactor is taken out and cooled to room temperature. The cooled solution is taken out and centrifuged for 10 minutes. The precipitate is washed with deionized water and repeated 5 times. The obtained solid is placed in an oven at 80°C and dried for 12 hours, and then calcined at 700°C for 1 hour to obtain tungsten oxide particles.

[0128] The specific surface area, D 90 , D 10 , D 50 The specific surface area, D 90 , D 10 and D 50 , the test results are shown in Table 1.

[0129] 3) The oxidation catalyst was prepared by loading palladium with the incipient wetness impregnation method. The specific steps included: adding 1.596 g of tungsten oxide to 1.5 ml of 0.04 mol / L palladium chloride solution, stirring for 1 h, standing for 12 h, drying at 110 °C, and treating at 400 °C for 3 h in a 30 ml / min H2 atmosphere.

[0130] Comparative Example 1

[0131] 1) Ammonium metatungstate is calculated as tungsten oxide, with a tungsten oxide concentration of 40 g / L, anhydrous oxalic acid concentration of 30 g / L, and a PVP concentration of 100 g / L with a molecular weight of 130,000 g / mol. Dissolve ammonium metatungstate, anhydrous oxalic acid, and PVP in deionized water to obtain 1 L of a mixed solution, put the mixed solution into a reactor with a polytetrafluoroethylene liner, and then put the reactor into an oven at 180°C for reaction for 18 hours;

[0132] 2) After the reaction is completed, take out the reactor and cool it to room temperature. Take out the cooled solution, centrifuge it for 10 minutes, wash the precipitate with deionized water, repeat 3 to 5 times, place the obtained solid in an oven at 80°C and dry it for 12 hours, then calcine it at 700°C for 1 hour to obtain tungsten oxide particles.

[0133] The specific surface area, D 90 , D 10 , D 50 The specific surface area, D 90 , D 10 and D 50 , the test results are shown in Table 1.

[0134] Figure 5 This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Comparative Example 1. The obtained tungsten oxide presents a micron-scale flaky structure.

[0135] 3) The oxidation catalyst was prepared by loading platinum with the incipient wetness impregnation method. The specific steps included: adding 1.573 g of tungsten oxide to 2 ml of 0.04 mol / L chloroplatinic acid solution and stirring for 1 h, standing for 12 h, and drying at 110°C, and treating at 300°C for 3 h in a 30 ml / min H2 atmosphere.

[0136] Comparative Example 3

[0137] According to the method of Example 1, except that in step 1), anhydrous oxalic acid is not added, and the other conditions are the same as those of Example 1; tungsten oxide particles are obtained.

[0138] Figure 6 This is a scanning electron microscope (SEM) image of the tungsten oxide particles prepared in Comparative Example 3, and the obtained tungsten oxide is in an obvious agglomerated state.

[0139] The specific surface area, D 90 , D 10 , D 50 The specific surface area, D 90 , D 10 and D 50 , the test results are shown in Table 1.

[0140] The oxidation catalyst was prepared by loading platinum using the incipient wetness impregnation method. The specific steps included: adding 1.573 g of tungsten oxide to 2 ml of 0.04 mol / L chloroplatinic acid solution and stirring for 1 h, standing for 12 h, and drying at 110°C, and treating at 300°C for 3 h in a 30 ml / min H2 atmosphere.

[0141] Comparative Example 4

[0142] The method of Example 1 is followed, except that in step 1), PVP is not added, and the remaining conditions are the same as those of Example 1; and there is no precipitation in the solution after the reaction.

[0143] Table 1

[0144]

[0145] Embodiment 8-14

[0146] Catalyst Evaluation:

[0147] The CO catalytic oxidation performance test was carried out in a fixed bed, with a test temperature range of 30°C to 400°C and a heating rate of 5°C / min. The raw gas composition was 0.5% CO, 10.5% O2, and 89% N2.

[0148] Total gas flow rate 50 ml / min, catalyst dosage 0.3 g, corresponding volume space velocity (GHSV) = 10000 ml g cat -1 ·h -1 The corresponding temperatures of catalyst CO oxidation T90 (temperature corresponding to 90% CO conversion rate) and T50 (temperature corresponding to 50% CO conversion rate) are shown in Table 2.

[0149] Figure 7 This is the relationship between CO oxidation conversion rate and temperature in Example 8.

[0150] Figure 8 This is the relationship between CO oxidation conversion rate and temperature in Example 9.

[0151] Fig. 9 This is the relationship between CO oxidation conversion rate and temperature in Example 10.

[0152] Fig.10 This is the relationship between CO oxidation conversion rate and temperature in Example 11.

[0153] Fig.11 This is the relationship between CO oxidation conversion rate and temperature in Example 12.

[0154] Fig.12 This is the relationship between CO oxidation conversion rate and temperature in Example 13;

[0155] Fig.13 This is the relationship between CO oxidation conversion rate and temperature in Comparative Example 2.

[0156] Table 2

[0157]

[0158] Comparative Example 6

[0159] The method of Example 8 is followed, except that tungsten oxide loaded with 3 wt% Pt is used to replace the catalyst prepared in Example 1;

[0160] The preparation method of tungsten oxide is as follows: ammonium metatungstate is directly calcined in a muffle furnace at 700° C. for 1 hour; the other conditions are the same as those in Example 8.

[0161] The catalyst was evaluated according to the method of Example 8. The results are as follows Fig.14 As shown, CO oxidation T90 is 173.4°C and T50 is 158.9°C.

[0162] According to the results of Example 8 and Comparative Example 6, it can be seen that the tungsten oxide particles prepared by the method of the present invention can reduce the amount of precious metal (Pt) while basically maintaining the catalytic performance.

[0163] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. Use of a catalytic oxidation catalyst in catalytic oxidation of CO, characterized in that: The catalyst comprises a carrier and an active component loaded on the carrier, wherein the carrier comprises ultrafine tungsten oxide particles, and the particle size distribution width of the ultrafine tungsten oxide particles is 1.0-3.0; 90 The value is 1-100μm, D 50 The value is 0.5-30μm, D 10 The value is 0.05-4μm; the particle size distribution width is calculated as (D 90 -D 10 ) / 2D 50 ; The active component is selected from one or more of Ru, Rh, Pd and Pt; The preparation method of ultrafine tungsten oxide particles includes: 1) subjecting a solution containing a template directing agent, a soluble tungsten salt, and a dispersing aid to a solvothermal reaction; 2) Separating the product obtained in step 1) to obtain a solid, drying and calcining to obtain tungsten oxide particles; the template directing agent is selected from one or more of oxalic acid, lactic acid, sulfuric acid, citric acid and ammonium acetate; the dispersing aid is selected from one or more of polyvinyl pyrrolidone, polyvinyl alcohol and polyethylene glycol; the mass ratio of the soluble tungsten salt is 0.5-5:1 based on tungsten oxide, and the mass ratio of the dispersing aid to the soluble tungsten salt is 0.2-2:1; the mass ratio of the template directing agent to the dispersing aid is 1:0.2-1; the mass of the soluble tungsten salt is calculated as tungsten oxide, and the concentration of the soluble tungsten salt in the solution is 5-50g / L; the solvent is water; the solvent thermal reaction temperature is 150-220°C, and the reaction time is 8-36h; the calcination temperature is 500-850°C, and the calcination time is 1-10h.

2. The use according to claim 1, wherein: The specific surface area of ​​the tungsten oxide particles is 1-100 m 2 / g.

3. The use according to claim 1, wherein: Based on the total mass of the catalyst, the active component content is 0.5-2.5wt%; and / or The carrier content is 97.5-99.5wt%.

4. The use according to claim 1, wherein: The preparation method of the catalytic oxidation catalyst comprises: (1) preparing a carrier according to the method for preparing ultrafine tungsten oxide particles; (2) The solution containing the active ingredient source is brought into contact with the carrier, the solvent is removed, and the solution is reduced.

5. The use according to claim 4, wherein: The concentration of the solution containing the active ingredient source is 0.01-0.5 mol / L; and / or The reduction conditions include: a reduction temperature of 200-450°C and a reduction time of 1-24h; and / or The active component source is selected from one or more soluble salts of active component elements.

6. The use according to claim 1, wherein: The application includes: catalytically oxidizing a raw gas containing CO and O2 in the presence of a catalyst.