A neutral aqueous electrolyte polyaniline-zinc battery

By using polyaniline cathode material with a high oxidation degree and amorphous structure and neutral aqueous electrolyte in polyaniline-zinc batteries, the problem of slow reaction in weakly acidic environments of polyaniline-zinc batteries has been solved, achieving high capacity, high energy density and long lifespan battery performance, and improving safety.

CN118539015BActive Publication Date: 2024-11-12SHANGHAI INVESTIGATION DESIGN & RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410393544.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-02
Publication Date
2024-11-12
Estimated Expiration
2044-04-02

AI Technical Summary

Technical Problem

The positive electrode material of existing polyaniline-zinc batteries is difficult to undergo rapid electrochemical oxidation-reduction reaction in a weakly acidic environment, which limits the improvement of battery performance. In addition, the acidity of traditional electrolytes is not suitable for zinc metal negative electrodes, posing a safety hazard.

Method used

High-oxidation-degree amorphous polyaniline is used as the positive electrode material, and lithium salt is added to the zinc salt electrolyte to adjust the pH of the electrolyte to the neutral range, forming a neutral aqueous electrolyte, which promotes the rapid redox reaction of the polyaniline positive electrode.

Benefits of technology

It improves the battery's specific capacity, energy density, and rate performance, extends battery life, and enhances battery safety, avoiding the risk of combustion and explosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118539015B_ABST
    Figure CN118539015B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of aqueous batteries, in particular to a neutral aqueous electrolyte polyaniline-zinc battery. The present invention adopts oxidized amorphous polyaniline as a positive electrode active material, adopts a mixed solution of lithium salt and zinc salt as an electrolyte, adopts zinc metal as a negative electrode, utilizes the reaction of oxidized amorphous polyaniline and lithium ions under neutral conditions as an electrochemical reaction of the positive electrode of the battery, and adopts a neutral aqueous electrolyte battery system of oxidized amorphous polyaniline||lithium / zinc ions||zinc, which can quickly carry out electrochemical redox reactions in a weakly acidic to neutral environment, overcomes the defect that the redox of existing polyaniline needs to be carried out smoothly under the condition of a lower pH value, and the provided neutral aqueous electrolyte polyaniline-zinc battery has a higher battery specific capacity, a greater energy density, a better rate performance, a longer battery life, and a higher safety due to the use of a weakly acidic to neutral aqueous electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aqueous batteries, in particular to a neutral aqueous electrolyte polyaniline-zinc battery. Background Art

[0002] Polyaniline-zinc ion battery is a low-cost aqueous battery with great application prospects. This battery uses polyaniline as the positive electrode material, zinc metal as the negative electrode material, and an aqueous solution of zinc salt as the electrolyte. This battery has the characteristics of high safety, high energy density and low cost. The use of aqueous solution as the electrolyte fundamentally eliminates the possibility of combustion and explosion. The zinc metal negative electrode has a theoretical specific capacity of 826mAh / g, and the positive electrode polyaniline can achieve a specific capacity of about 100mAh / g at a lower current and density (not higher than 50mA / g), and has an average discharge voltage of about 1.0-1.1V. This allows the polyaniline zinc ion battery to achieve an energy density of 50-80Wh / kg. In addition, since both polyaniline and zinc are low-value materials and an aqueous solution is used as the electrolyte, polyaniline-zinc ion has good economy.

[0003] Positive and negative electrode reactions of polyaniline-zinc battery:

[0004] positive electrode:

[0005]

[0006] negative electrode:

[0007]

[0008] Generally speaking, the redox of polyaniline can only proceed smoothly under the condition of a relatively low pH value (generally, pH ≤ 4). Although the aqueous solutions of common water-soluble zinc salts (such as zinc sulfate, zinc chloride, zinc trifluoromethanesulfonate, etc.) generally have a certain weak acidity (pH = 4 to 7), such acidity is not enough to cause the electrochemical redox reaction of the polyaniline positive electrode to occur quickly. In addition, since the zinc at the negative electrode can react with the acid in the electrolyte to generate hydrogen, the pH value of the electrolyte cannot be lowered by adding acid to the electrolyte.

[0009] In summary, the cathode material and its supporting electrolyte system are important factors that restrict the performance of polyaniline-zinc batteries. Co-optimizing the polyaniline and electrolyte system so that the cathode material can undergo rapid electrochemical redox reactions in a weakly acidic to neutral environment is the key to improving the performance of such batteries. Summary of the invention

[0010] In view of the problems existing in the prior art, the present invention provides a neutral aqueous electrolyte polyaniline-zinc battery, which adds a certain amount of lithium salt to the zinc salt electrolyte to cause the polyaniline positive electrode to rapidly undergo an electrochemical redox reaction, and simultaneously uses a polyaniline base (intrinsic polyaniline) with a non-crystalline structure with a high oxidation degree as the positive electrode material, thereby improving the battery specific capacity, energy density and rate performance, extending the battery life, and the safety of the neutral electrolyte is also improved.

[0011] To achieve this object, the present invention adopts the following technical solutions:

[0012] The first aspect of the present invention provides a neutral aqueous electrolyte polyaniline-zinc battery, comprising a positive electrode, an electrolyte and a negative electrode; the positive electrode comprises oxidized amorphous polyaniline, a conductive agent and a binder; the negative electrode is zinc metal; the components of the electrolyte include zinc salt and lithium salt, and the zinc salt and the lithium salt have the same anion.

[0013] In some embodiments of the present invention, the oxidized amorphous polyaniline is an intrinsic oxidized amorphous polyaniline, and its structural formula is shown in the following formula (I):

[0014]

[0015] In some embodiments of the present invention, the conductive agent is selected from any one of conductive graphite, carbon nanotubes, conductive carbon black, graphene, and carbon fiber.

[0016] In some embodiments of the present invention, the binder is polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE).

[0017] In some embodiments of the present invention, the mass ratio of the oxidized amorphous polyaniline, the conductive agent and the binder is 85-93:5-10:2.5-5.

[0018] In some embodiments of the present invention, the positive electrode loading is 5 to 25 mg / cm 2 .

[0019] In some embodiments of the present invention, the concentration of the zinc salt in the electrolyte is in the range of 0.1 to 5 mol / L or saturated concentration.

[0020] In some embodiments of the present invention, the concentration of the lithium salt in the electrolyte is in the range of 0.1 to 10 mol / L.

[0021] In some embodiments of the present invention, the components of the electrolyte further include a pH adjuster, a surfactant, an organic solvent and water.

[0022] In some embodiments of the present invention, the pH of the electrolyte is 5.5-7.5.

[0023] In some embodiments of the present invention, the anions of the zinc salt and the lithium salt are selected from any one of chloride, sulfate, trifluoromethylsulfonate and acetate.

[0024] In some embodiments of the present invention, the zinc metal is selected from zinc foil.

[0025] The second aspect of the present invention provides a method for preparing the above-mentioned neutral aqueous electrolyte polyaniline-zinc battery, comprising the following steps:

[0026] (1) fully mixing and grinding polyaniline, a conductive agent and a binder powder according to a mass ratio to obtain a mixed positive electrode material;

[0027] (2) adding the mixed positive electrode material obtained in step (1) into N-methylpyrrolidone and stirring to obtain a slurry;

[0028] (3) coating the slurry obtained in step (2) on a current collector and vacuum drying to obtain a positive electrode material;

[0029] (4) Using the positive electrode material obtained in step (3) as the positive electrode and zinc metal as the negative electrode, assembling the positive electrode, the separator and the negative electrode in sequence, and adding an electrolyte to obtain a neutral aqueous electrolyte polyaniline-zinc battery.

[0030] In some embodiments of the present invention, the mass fraction of the mixed positive electrode material in the slurry obtained in step (2) is 10 wt % to 25 wt %.

[0031] In some embodiments of the present invention, the coating in step (3) is blade coating.

[0032] In some embodiments of the present invention, the vacuum drying temperature in step (3) is 80-120°C.

[0033] In some embodiments of the present invention, the current collector in step (3) is selected from any one of stainless steel foil, stainless steel mesh, titanium foil or titanium mesh.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] 1. The neutral aqueous electrolyte polyaniline-zinc battery provided by the present invention uses amorphous polyaniline as the positive electrode active material, a mixed solution of lithium salt and zinc salt as the electrolyte, and zinc metal as the negative electrode. The battery has higher specific capacity, greater energy density, and better rate performance.

[0036] 2. The neutral aqueous electrolyte polyaniline-zinc battery provided by the present invention has a longer life. Under the charge and discharge condition of 4C, the remaining capacity is about 96.9% after 500 charge and discharge cycles, and the remaining capacity is 93.7% after 2000 charge and discharge cycles.

[0037] 3. The neutral aqueous electrolyte polyaniline-zinc battery provided by the present invention adopts a weakly acidic to neutral aqueous electrolyte with a pH of 5.5 to 7.5, is weakly corrosive, and does not have the risk of combustion and explosion. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 The test results of the charge and discharge capacity of the neutral aqueous electrolyte polyaniline-zinc battery provided in Example 1 of the present invention.

[0039] Figure 2 The test results of the cycle life of the neutral aqueous electrolyte polyaniline-zinc battery prepared in Example 1 of the present invention are shown. DETAILED DESCRIPTION

[0040] The neutral aqueous electrolyte polyaniline-zinc battery of the present invention is described in detail below.

[0041] The specific technical solutions are as follows:

[0042] The first aspect of the present invention provides a neutral aqueous electrolyte polyaniline-zinc battery, comprising a positive electrode, an electrolyte and a negative electrode; the positive electrode comprises oxidized amorphous polyaniline, a conductive agent and a binder; the negative electrode is zinc metal; the components of the electrolyte include zinc salt and lithium salt, and the zinc salt and the lithium salt have the same anion.

[0043] In addition to undergoing electrochemical oxidation reactions in the form of protonation under acidic conditions, polyaniline can also undergo redox reactions in the form of lithium ion doping. By adding a certain amount of lithium salt to the zinc salt electrolyte, the polyaniline positive electrode can rapidly undergo electrochemical redox reactions, thereby overcoming the defect that the existing redox of polyaniline requires a relatively low pH value (generally pH ≤ 4) to proceed smoothly, and enabling the positive electrode material to rapidly undergo electrochemical redox reactions in a weakly acidic to neutral environment.

[0044] In the present invention, the reaction equation of the electrochemical redox reaction of the polyaniline positive electrode is as follows:

[0045]

[0046] General polyaniline materials have a relatively compact crystalline structure, which has a strong inhibitory effect on the diffusion of lithium ions. In the present invention, oxidized amorphous polyaniline is selected as the positive electrode material. The X-ray diffraction pattern of the oxidized amorphous polyaniline has no diffraction peaks, and the amorphous structure is conducive to the diffusion of ions inside the electrode, and has better electrochemical reaction kinetics. When the electrode material loading is ≥5mg / cm 2 When the amorphous polyaniline electrode is oxidized under the same conditions, it has a higher specific capacitance and better rate performance. Preferably, the positive electrode specific capacity is controlled at 2 to 5 mAh / cm 2 within the range.

[0047] The X-ray diffraction pattern of the oxidized amorphous polyaniline has no diffraction peak, which means that there is no obvious diffraction peak within the scanning range of XRD, that is, the oxidized amorphous polyaniline has an amorphous structure. The molecular chain of the intrinsic oxidized amorphous polyaniline is linear. The oxidation degree of the oxidized amorphous polyaniline is a completely oxidized state.

[0048] The density of ordinary polyaniline-carbon black pressed electrode prepared with ordinary polyaniline is generally 1.0-1.2 g / cm -3 The density of amorphous polyaniline-carbon black electrode prepared by amorphous polyaniline can reach 1.4-1.6 g / cm -3 .

[0049] In some embodiments of the present invention, the oxidized amorphous polyaniline is an intrinsic oxidized amorphous polyaniline, and its structural formula is shown in the following formula (I):

[0050]

[0051] In some embodiments of the present invention, the method for preparing oxidized amorphous polyaniline comprises the following steps:

[0052] (1) adding a bridging molecule or a precursor of a bridging molecule to an aniline solution to obtain a trimer solution;

[0053] (2) subjecting the trimer solution to an oxidative polymerization reaction to obtain a polyaniline-bridging molecule hybrid;

[0054] (3) The polyaniline-bridging molecule hybrid is treated with an alkaline solution to obtain an intrinsically oxidized amorphous polyaniline.

[0055] Preferably, the aniline solution also includes an acid solution, and the acid solution is selected from a medium-strong acid solution or a strong acid solution; preferably, the hydrogen ion concentration of the acid solution is 0.2-2 mol / L; preferably, the concentration of aniline monomer in the aniline solution is 0.1-2 mol / L, and is not higher than the hydrogen ion concentration of the acid solution in the aniline solution; preferably, the bridging molecule is selected from a dibasic weak acid, such as tungstic acid, molybdic acid, terephthalic acid, etc.; the molar ratio of the bridging molecule to the aniline monomer is 1±0.02:2 mol / mol; the molar ratio of the bridging molecule formed by the precursor of the bridging molecule to the aniline monomer is 1±0.02:2 mol / mol.

[0056] In some embodiments of the present invention, the conductive agent includes but is not limited to conductive graphite, carbon nanotubes, conductive carbon black, graphene, and carbon fiber; the conductive carbon black is preferably Ketjen black.

[0057] In some embodiments of the present invention, the binder is polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE).

[0058] In some embodiments of the present invention, the mass ratio of the oxidized amorphous polyaniline, the conductive agent and the binder is 85-93:5-10:2.5-5, preferably 90:7.5:2.5.

[0059] In some embodiments of the present invention, the positive electrode loading is 5 to 25 mg / cm 2 , can be 5~10mg / cm 2 , 10~15mg / cm 2 , 15~20mg / cm 2 , or 20-25 mg / cm 2 , preferably 10 to 15 mg / cm 2 .

[0060] In some embodiments of the present invention, the concentration of the zinc salt in the electrolyte is in the range of 0.1 to 5 mol / L or saturated concentration. When the saturated concentration of the zinc salt is greater than 5 mol / L, it is 0.1 to 5 mol / L, and when the saturated concentration of the zinc salt is less than 5 mol / L, it is 0.1 mol / L to saturated concentration.

[0061] In some embodiments of the present invention, the concentration range of the lithium salt in the electrolyte is 0.1-10 mol / L, which can be 0.1-1 mol / L, 1-2 mol / L, 2-3 mol / L, 3-4 mol / L, 4-5 mol / L, 5-6 mol / L, 6-7 mol / L, 7-8 mol / L, 8-9 mol / L, and can also be 9-10 mol / L, preferably 5-8 mol / L.

[0062] In some embodiments of the present invention, the pH of the electrolyte is 5.5-7.5, and may be 5.5-6.0, 6.0-6.5, 6.5-7.0, or 7.0-7.5.

[0063] In some embodiments of the present invention, the anions of the zinc salt and the lithium salt are selected from any one of chloride, sulfate, trifluoromethanesulfonate, acetate, etc. For example, zinc chloride / lithium, zinc sulfate / lithium, zinc tetrafluoroborate / lithium, zinc trifluoromethanesulfonate / lithium, zinc acetate / lithium, etc.

[0064] In some embodiments of the present invention, the zinc metal is selected from zinc foil.

[0065] In some embodiments of the present invention, the components of the electrolyte further include a pH regulator, a surfactant, an organic solvent and water. Preferably, the pH regulator includes but is not limited to sodium citrate, sodium acetate, and tetraethylammonium hydroxide; preferably, the surfactant includes but is not limited to sodium dodecyl sulfonate (SDBS), tetraethylammonium bromide (TEABr), hexadecyltrimethylammonium bromide (CTAB), dodecyldimethylbenzylammonium chloride (DDBAC), dodecyltrimethylammonium chloride (DTAC), benzyltrimethylammonium chloride (TMBAC), and tetrabutylammonium sulfate (TBA2SO4); preferably, the organic solvent includes but is not limited to methanol, ethanol, propanol, isopropanol, ethylene glycol, glycerol, polyethylene glycol, N-methylpyrrolidone (NMP), dimethyl sulfoxide (DMSO), and N,N-dimethylacetamide (DMF).

[0066] In some embodiments of the present invention, the molar concentration of the pH regulator in the electrolyte is 0-0.5 mol / L, which can be 0-0.1 mol / L, 0.1-0.2 mol / L, 0.2-0.3 mol / L, 0.3-0.4 mol / L, or 0.4-0.5 mol / L, preferably 0.1 mol / L.

[0067] In some embodiments of the present invention, the mass concentration of the surfactant in the electrolyte is 0-0.5wt%, which may be 0-0.1wt%, 0.1-0.2wt%, 0.2-0.3wt%, 0.3-0.4wt%, or 0.4-0.5wt%, preferably 0.15wt%.

[0068] In some embodiments of the present invention, the mass fraction of the organic solvent in the electrolyte is 0-10%.

[0069] The second aspect of the present invention provides a method for preparing the above-mentioned neutral aqueous electrolyte polyaniline-zinc battery, comprising the following steps:

[0070] (1) fully mixing and grinding polyaniline, a conductive agent and a binder powder according to a mass ratio to obtain a mixed positive electrode material;

[0071] (2) adding the mixed positive electrode material obtained in step (1) into N-methylpyrrolidone and stirring to obtain a slurry;

[0072] (3) coating the slurry obtained in step (2) on a current collector and vacuum drying to obtain a positive electrode material;

[0073] (4) Using the positive electrode material obtained in step (3) as the positive electrode and zinc metal as the negative electrode, assembling the positive electrode, the separator and the negative electrode in sequence, and adding an electrolyte to obtain a neutral aqueous electrolyte polyaniline-zinc battery.

[0074] In some embodiments of the present invention, the mass fraction of the mixed positive electrode material in the slurry obtained in step (2) is 10wt% to 25wt%, can be 10wt% to 15wt%, 15wt% to 20wt%, or 20wt% to 25wt%, preferably 15wt%.

[0075] In some embodiments of the present invention, the coating in step (3) is scraping.

[0076] In some embodiments of the present invention, the vacuum drying temperature in step (3) is 80-120°C, which can be 80-85°C, 85-90°C, 90-95°C, 95-100°C, 100-105°C, 105-110°C, 110-115°C, or 115-120°C.

[0077] In some embodiments of the present invention, the current collector in step (3) includes but is not limited to stainless steel foil, stainless steel mesh, titanium foil or titanium mesh.

[0078] The specific embodiments of the present invention are further described in detail below in conjunction with preferred embodiments. When the embodiments provide numerical ranges, it should be understood that, unless otherwise specified in the present invention, the two endpoints of each numerical range and any numerical value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those generally understood by those skilled in the art. In addition to the specific methods, equipment, and materials used in the embodiments, as those skilled in the art grasp the prior art and record the present invention, any methods, equipment, and materials of the prior art similar or equivalent to the methods, equipment, and materials described in the embodiments of the present invention can also be used to realize the present invention.

[0079] It should be noted that the oxidized amorphous polyaniline used in the following examples is intrinsic oxidized amorphous polyaniline prepared according to the preparation method of Example 9 of patent document CN117586500A.

[0080] Example 1

[0081] A method for preparing a neutral aqueous electrolyte polyaniline-zinc battery comprises the following steps:

[0082] (1) Preparation of positive electrode material: Oxidized amorphous polyaniline, conductive agent (ketjen black), and binder (PVDF) powders were fully mixed and ground in a mass ratio of 90:7.5:2.5 to obtain a mixed positive electrode material;

[0083] (2) taking a mixed positive electrode material at a ratio of 15 wt %, adding it to N-methylpyrrolidone (NMP) and stirring it thoroughly to form a slurry;

[0084] (3) The slurry was coated on a stainless steel foil by a doctor blade method and then placed in a vacuum oven and dried at 80°C to obtain a positive electrode. The loading of the obtained electrode was 7.5±0.5 mg / cm 2 .

[0085] (4) Battery assembly: Using the positive electrode obtained in step (3) and zinc foil as the negative electrode, the positive electrode, the separator and the negative electrode are sequentially loaded into a button battery with a specification of 2032, and an electrolyte is added. The electrolyte is an aqueous solution of lithium sulfate (1.25 mol / L), zinc sulfate (1.5 mol / L), tetraethylammonium bromide (0.15 wt%) and methanol (10 wt%) (the pH value of the solution is adjusted to 7.0 with 0.1 mol / L sodium citrate solution), and a neutral aqueous electrolyte polyaniline-zinc battery is obtained.

[0086] Example 2

[0087] A method for preparing a neutral aqueous electrolyte polyaniline-zinc battery comprises the following steps:

[0088] (1) Preparation of positive electrode material: Oxidized amorphous polyaniline, conductive agent (ketjen black), and binder (PVDF) powders were fully mixed and ground in a mass ratio of 90:7.5:2.5 to obtain a mixed positive electrode material.

[0089] (2) Take a mixed positive electrode material at a ratio of 15 wt %, add it to N-methylpyrrolidone (NMP), and stir it thoroughly to form a slurry.

[0090] (3) The slurry was coated on a stainless steel foil by a doctor blade method and then placed in a vacuum oven and dried at 80°C to obtain a positive electrode material. The loading amount of the obtained positive electrode material was 10±0.5 mg / cm 2 .

[0091] (4) Battery assembly: Using the positive electrode obtained in step (3) and zinc foil as the negative electrode, the positive electrode, the separator and the negative electrode are sequentially loaded into a button battery with a specification of 2032, and an electrolyte is added. The electrolyte is an aqueous solution of lithium sulfate (1.25 mol / L), zinc sulfate (1.5 mol / L), tetraethylammonium bromide (0.15 wt%) and methanol (10 wt%) (the pH value of the solution is adjusted to 7.0 with 0.1 mol / L sodium citrate solution), and a neutral aqueous electrolyte polyaniline-zinc battery is obtained.

[0092] Example 3

[0093] A method for preparing a neutral aqueous electrolyte polyaniline-zinc battery comprises the following steps:

[0094] (1) Preparation of positive electrode material: Oxidized amorphous polyaniline, conductive agent (ketjen black), and binder (PVDF) powders were fully mixed and ground in a mass ratio of 90:7.5:2.5 to obtain a mixed positive electrode material.

[0095] (2) Take a mixed positive electrode material at a ratio of 15 wt %, add it to N-methylpyrrolidone (NMP), and stir it thoroughly to form a slurry.

[0096] (3) The slurry was coated on a stainless steel foil by a doctor blade method and then placed in a vacuum oven and dried at 80°C to obtain a positive electrode material. The loading amount of the obtained positive electrode material was 15±0.5 mg / cm 2 .

[0097] (4) Battery assembly: Using the positive electrode obtained in step (3) and zinc foil as the negative electrode, the positive electrode, the separator and the negative electrode are sequentially loaded into a button battery with a specification of 2032, and an electrolyte is added. The electrolyte is an aqueous solution of lithium sulfate (1.25 mol / L), zinc sulfate (1.5 mol / L), tetraethylammonium bromide (0.15 wt%) and methanol (10 wt%) (the pH value of the solution is adjusted to 7.0 with 0.1 mol / L sodium citrate solution), and a neutral aqueous electrolyte polyaniline-zinc battery is obtained.

[0098] Comparative Example 1

[0099] Except that common polyaniline is used as the positive electrode material, the rest is the same as in Example 1.

[0100] Comparative Example 2

[0101] The same procedures as in Example 1 were followed except that the lithium chloride concentration in the electrolyte was reduced to 1 mol / L and the zinc chloride concentration was increased to 2.25 mol / L.

[0102] Battery performance test

[0103] 1. Charge and discharge capacity test

[0104] Taking the mass of the battery positive electrode as a reference, the neutral aqueous electrolyte polyaniline-zinc batteries prepared in Examples 1 to 3 were respectively subjected to constant current charge and discharge tests at three different current densities of 100 mA / g, 200 mA / g and 500 mA / g. The charge and discharge voltage range was 0.4 to 1.5 V. The test results are shown in Table 1 below.

[0105] Table 1

[0106]

[0107] From the test results in Table 1, it can be seen that the electrode thickness (loading amount) has a certain influence on the performance of oxidized amorphous polyaniline, but the influence is not significant; under the condition of neutral lithium-rich electrolyte, compared with ordinary polyaniline, oxidized amorphous polyaniline has higher electrochemical activity, which is specifically reflected in higher specific capacity and better rate performance; the concentration of lithium ions in the electrolyte has a relatively significant effect on the electrochemical performance of oxidized amorphous polyaniline.

[0108] 2. Energy density

[0109] The energy is calculated by integrating the product of voltage and current (power): E = Σ(U × I) or E = I∫U(t)dt, where E is energy, U is voltage, I is current, and t is time. According to calculations, the theoretical specific energy of the neutral aqueous electrolyte polyaniline-zinc battery provided in Example 1 under 1C conditions is 115wh / kg.

[0110] like Figure 1 As shown, under 1C charge and discharge conditions, the positive electrode specific capacity of the neutral aqueous electrolyte polyaniline-zinc battery provided in Example 1 can reach more than 200 mAh / g.

[0111] 3. Cycle life test

[0112] Under the charge and discharge condition of 4C, the neutral aqueous electrolyte polyaniline-zinc battery prepared in Example 1 was subjected to multiple charge and discharge cycles, and the capacity change of the battery after each cycle was recorded. The results are as follows: Figure 2 shown.

[0113] Depend on Figure 2 It can be seen that the neutral aqueous electrolyte polyaniline-zinc battery prepared in Example 1 has a capacity remaining of about 96.9% after 500 charge and discharge cycles, about 94.6% after 1000 cycles, about 93.9% after 1500 cycles, and 93.7% after 2000 cycles.

[0114] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.

Claims

1. A neutral aqueous electrolyte polyaniline-zinc battery, characterized in that: The invention comprises a positive electrode, an electrolyte and a negative electrode; the positive electrode comprises oxidized amorphous polyaniline, a conductive agent and a binder; the negative electrode is zinc metal; the components of the electrolyte comprise zinc salt and lithium salt, and the zinc salt and the lithium salt have the same anion.

2. The neutral aqueous electrolyte polyaniline-zinc battery according to claim 1, characterized in that: Includes one or more of the following characteristics: (a) The oxidized amorphous polyaniline is an intrinsic oxidized amorphous polyaniline, and its structural formula is shown in the following formula (I): (b) the conductive agent is selected from any one of conductive graphite, carbon nanotubes, conductive carbon black, graphene, and carbon fiber; (c) the binder is polyvinylidene fluoride or polytetrafluoroethylene; (d) the mass ratio of the oxidized amorphous polyaniline, the conductive agent and the binder is 85-93:5-10:2.5-5; (e) The positive electrode loading is 5 to 25 mg / cm 2 .

3. The neutral aqueous electrolyte polyaniline-zinc battery according to claim 1, comprising one or more of the following features: (f) the concentration of zinc salt in the electrolyte is in the range of 0.1 to 5 mol / L or saturated concentration; (g) the concentration of lithium salt in the electrolyte is in the range of 0.1 to 10 mol / L; (h) The electrolyte further comprises a pH regulator, a surfactant, an organic solvent and water; (i) the pH of the electrolyte is 5.5 to 7.5; (j) the anions of the zinc salt and the lithium salt are selected from any one of chloride, sulfate, trifluoromethylsulfonate and acetate; (k) The zinc metal is selected from zinc foil.

4. The neutral aqueous electrolyte polyaniline-zinc battery according to claim 2, wherein the conductive carbon black is selected from Ketjen black.

5. The neutral aqueous electrolyte polyaniline-zinc battery according to claim 3, comprising one or more of the following features: (h1) the pH adjuster is selected from any one of sodium citrate, sodium acetate, and tetraethylammonium hydroxide; (h2) the surfactant is selected from any one of sodium dodecyl sulfonate, tetraethylammonium bromide, hexadecyltrimethylammonium bromide, dodecyldimethylbenzylammonium chloride, dodecyltrimethylammonium chloride, benzyltrimethylammonium chloride and tetrabutylammonium sulfate; (h3) the organic solvent is selected from any one of methanol, ethanol, propanol, isopropanol, ethylene glycol, glycerol, polyethylene glycol, N-methylpyrrolidone, dimethyl sulfoxide, and N,N-dimethylacetamide; (h4) the molar concentration of the pH regulator in the electrolyte is 0 to 0.5 mol / L; (h5) The mass concentration of the surfactant in the electrolyte is 0 to 0.5 wt %; (h6) The mass fraction of the organic solvent in the electrolyte is 0 to 10%.

6. A method for preparing a neutral aqueous electrolyte polyaniline-zinc battery according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) fully mixing and grinding polyaniline, a conductive agent and a binder powder according to a mass ratio to obtain a mixed positive electrode material; (2) adding the mixed positive electrode material obtained in step (1) into N-methylpyrrolidone and stirring to obtain a slurry; (3) coating the slurry obtained in step (2) on a current collector and vacuum drying to obtain a positive electrode material; (4) Using the positive electrode material obtained in step (3) as the positive electrode and zinc metal as the negative electrode, assembling the positive electrode, the separator and the negative electrode in sequence, and adding an electrolyte to obtain a neutral aqueous electrolyte polyaniline-zinc battery.

7. The method for preparing a neutral aqueous electrolyte polyaniline-zinc battery according to claim 6, characterized in that: The mass fraction of the mixed positive electrode material in the slurry obtained in step (2) is 10wt% to 25wt%.

8. The method for preparing a neutral aqueous electrolyte polyaniline-zinc battery according to claim 6, characterized in that: The coating in step (3) is scraping.

9. The method for preparing a neutral aqueous electrolyte polyaniline-zinc battery according to claim 6, characterized in that: The vacuum drying temperature in step (3) is 80-120°C.

10. The method for preparing a neutral aqueous electrolyte polyaniline-zinc battery according to claim 6, characterized in that: The current collector in step (3) is selected from stainless steel foil, stainless steel mesh, titanium foil or titanium mesh.