A method for preparing composite air filter material
Through low-temperature electric field pretreatment of polylactic acid materials and laser plasma beam etching technology, combined with the addition of electrospinned nanofiber membrane layer, the problems of non-degradability and insufficient performance of the air filter element material are solved, and efficient and environmentally friendly air filtration is achieved Material.
Patent Information
- Application Number
- CN202411017978.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing air filter material is non-degradable, making it difficult to dispose of waste, and traditional methods are difficult to achieve high efficiency, low resistance, anti-aging, ultraviolet rays, moisture resistance and temperature resistance requirements.
Modified polylactic acid is used to form after low-temperature electric field pretreatment, and a composite fiber web is formed by laser and plasma beam etching, and a nanofiber membrane layer is added to electrospinning technology to form a highly efficient composite air filter material.
It achieves high efficiency, low resistance, anti-aging, UV, moisture and high temperature air filtration performance, while the material is biodegradable.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of filtration and separation, and in particular relates to a method for preparing a composite air filter material. Background Art
[0002] With the rapid economic development, the use of air filters as disposable consumables is increasing, both in the industrial and civilian fields. The huge consumption of filter elements brings with it the thorny problem of how to deal with discarded filter elements. Since the core components of air filters - filter materials are mostly non-degradable materials, such as polypropylene, polyester, polyethylene and glass fiber, and it is currently difficult to recycle and reuse these materials separately. In the past, the common treatment method was to crush and then incinerate or landfill, but both methods would harm the environment. Incineration would increase the emission of pollutants such as carbon dioxide, sulfur dioxide, nitrogen oxides and smoke, and landfill would increase the soil pollution load, because the degradation cycle of polypropylene, polyester, polyethylene, etc. is hundreds of years, and the degradation cycle of glass fiber is millions of years.
[0003] With the proposal of establishing and improving a green, low-carbon, circular development economic system, various regions have successively proposed banning the production, sale and use of non-degradable plastic products and vigorously promoting the use of biodegradable materials.
[0004] In addition to the requirement of being biodegradable, high-efficiency air filter materials should also have the characteristics of high efficiency, low resistance, anti-aging, anti-ultraviolet, anti-humidity, temperature resistance and strength. At present, traditional preparation methods and existing biodegradable materials are difficult to achieve these requirements.
[0005] Therefore, providing a method for preparing a composite air filter material so that it has the above-mentioned excellent properties and is biodegradable is a technical problem to be solved urgently in the art. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing a composite air filter material.
[0007] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a composite air filter material, comprising the following steps:
[0008] S1. Mix polylactic acid, thiophenedicarboxylic acid, halogenated phenol, aromatic guanidine, palm kernel oil diethanolamide, maleic anhydride and polyvinyl pyrrolidone in a reaction kettle, stir and react at a temperature of 20 to 30°C, then add tris(2,4-di-tert-butylphenyl)phosphite and 2-(2-hydroxy-5-methylphenyl)benzotriazole, stir and react at a temperature of 40 to 60°C to obtain modified polylactic acid;
[0009] S2, pre-treating the modified polylactic acid in a low temperature (-60~-40°C, voltage of 20~40kV) electric field for 1~3h;
[0010] S3, drying the pretreated modified polylactic acid in a vacuum drying oven at a temperature of 80-90°C for 6-10 hours;
[0011] S4, the dried modified polylactic acid is fed from the hopper into a screw extruder and heated to form a melt with good fluidity, and the die head heating temperature is set to 190-260°C;
[0012] S5, the melt is extruded from the spinneret hole to form filaments with a diameter of 4-6 μm, which are cooled by air to form a fiber web on a web laying machine, and the fiber web is reinforced by a hot rolling mill to form a substrate with a basis weight of 50-70 g / m 2 ;
[0013] S6, using laser and plasma beam to etch and trim the surface of the substrate fiber at the same time, the angle between the laser and plasma beam is 30° to 45°;
[0014] S7, dissolving the modified polylactic acid in a mixed solvent, wherein the mixed solvent includes dioxane, acetone, dimethylformamide, dichloroethane and dichloromethane, and stirring and dissolving at 40-50° C. to form a spinning solution;
[0015] S8, the spinning solution is electrostatically pulled to form a nanofiber membrane layer with an average diameter of 0.5-0.7 μm on the substrate etched and trimmed in step S6, with a quantitative weight of 1-5 g / m 2 ;
[0016] S9, the substrate with the nanofiber membrane layer obtained in step S8 is reinforced by a hot rolling mill to form a composite air filter material.
[0017] Further, in step S1, 30-50 parts of polylactic acid chips, 5-10 parts of thiophenedicarboxylic acid, 5-10 parts of halogenated phenol, 3-5 parts of aromatic guanidine, 15-20 parts of palm kernel oil diethanolamide, 5-10 parts of maleic anhydride, and 3-5 parts of polyvinyl pyrrolidone are weighed by weight, mixed and placed in a reaction kettle, stirred and reacted at a temperature of 20-30° C. for 1-3 hours, and then 5-10 parts of tris(2,4-di-tert-butylphenyl)phosphite and 5-10 parts of 2-(2-hydroxy-5-methylphenyl)benzotriazole are added, and stirred and reacted at a temperature of 40-60° C. for 4-6 hours.
[0018] Furthermore, the polylactic acid has a melting point of 140-160°C, a melt index of 30-60 g / 10 min, and a molecular weight of 7×10 4 ~9×10 4, density is 1.20~1.25g / cm 3 .
[0019] Furthermore, in step S6, the pulse energy of the laser is 1 to 10 fs, and the time is 1 to 3 min; the discharge power of the plasma beam is 200 to 400 W, the voltage applied to the upper and lower positive and negative electrodes is 100 to 200 V, the time is 1 to 3 min, and the frequency of the excitation source is 40 to 100 KHz.
[0020] Furthermore, in step S7, the mass ratio of dioxane, acetone, dimethylformamide, dichloroethane and dichloromethane in the mixed solvent is: (10-30): (30-40): (10-20): (10-20): (10-20).
[0021] Furthermore, in step S7, the spinning solution concentration is 9% to 12%.
[0022] Further, in step S8, the electrostatic traction voltage is 15-25 kV, and the receiving distance is 15-20 cm.
[0023] The beneficial effects of the present invention are:
[0024] (1) The existing modified polylactic acid focuses on improving the toughness and temperature resistance of polylactic acid, while the present invention independently modifies polylactic acid to have anti-aging, anti-ultraviolet, high temperature resistance, high strength and other properties, thereby greatly extending the service life of the air filter material.
[0025] (2) The composite air filter material of the present invention is pretreated in a low-temperature electric field before the modified polylactic acid is melted, so that the modified polylactic acid molecular chains are oriented and dipole polarized, thereby enhancing the bonding strength between the molecular chains and greatly improving the tensile strength of the substrate after molding.
[0026] (3) The present invention innovatively uses laser and plasma beams at a certain angle to etch the surface of the substrate fiber at the same time. Compared with the previous etching using laser or plasma beam alone, it has achieved unexpected results, making the microstructure of the fiber surface after etching more conducive to improving hydrophobicity. Moreover, it is difficult to obtain a better hydrophobic etching effect when the angle between the laser and plasma beam is less than 30° or more than 45°.
[0027] (4) The present invention identifies the key conditions for improving the filtration performance of composite air filter materials and achieves high efficiency and low resistance by controlling the quantitative amount of electrospun nanofiber membranes.
[0028] It can be seen that the composite air filter material obtained by the method of the present invention is suitable for high-efficiency air filtration in various occasions. While having the characteristics of high efficiency and low resistance, anti-aging, UV resistance, moisture resistance, high temperature resistance and high strength, it can also be completely degraded into carbon dioxide and water under soil or composting conditions after use. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the best embodiment.
[0030] Example 1
[0031] A method for preparing a composite air filter material comprises the following steps:
[0032] S1. According to weight, 50 parts of polylactic acid chips, 5 parts of thiophenedicarboxylic acid, 5 parts of halogenated phenol, 3 parts of aromatic guanidine, 15 parts of palm kernel oil diethanolamide, 5 parts of maleic anhydride, and 3 parts of polyvinyl pyrrolidone were weighed and mixed in a reaction kettle, stirred and reacted at a temperature of 25°C for 2h, and then 5 parts of tris(2,4-di-tert-butylphenyl)phosphite and 5 parts of 2-(2-hydroxy-5-methylphenyl)benzotriazole were added, stirred and reacted at a temperature of 50°C for 5h to obtain modified polylactic acid;
[0033] S2, pre-treating the modified polylactic acid in an electric field at -40°C and a voltage of 20 kV for 2 h;
[0034] S3, drying the pretreated modified polylactic acid in a vacuum drying oven at a temperature of 90° C. for 6 h;
[0035] S4, the dried modified polylactic acid is fed from the hopper into a screw extruder and heated to form a melt with good fluidity, and the die head heating temperature is set to 220°C;
[0036] S5, the melt is extruded from the spinneret hole to form filaments with a diameter of 5 μm, which are cooled by air and then formed into a fiber web on a web laying machine. The fiber web is reinforced by a hot rolling mill to form a substrate with a basis weight of 60 g / m 2 ;
[0037] S6. The surface of the substrate fiber is etched and trimmed by using laser and plasma beams at the same time. The angle between the laser and plasma beams is 45°. The pulse energy of the laser is 5fs and the duration is 3min. The discharge power of the plasma beam is 300W. The voltage applied to the upper and lower positive and negative electrodes is 150V and the duration is 3min. The frequency of the excitation source is 40KHz.
[0038] S7, dissolving the modified polylactic acid in a mixed solvent, wherein the mixed solvent includes dioxane, acetone, dimethylformamide, ethylene dichloride and dichloromethane, wherein the mass ratio of dioxane, acetone, dimethylformamide, ethylene dichloride and dichloromethane is 10: 30: 20: 10: 20, and stirring and dissolving at 45° C. to form a spinning solution; the spinning solution concentration is 10%;
[0039] S8, the spinning solution is electrostatically pulled to form a nanofiber membrane layer with an average diameter of 0.7 μm on the substrate etched and trimmed in step S6, with a quantitative weight of 3 g / m 2 ; The electrostatic traction voltage is 20kV and the receiving distance is 20cm;
[0040] S9, the substrate with the nanofiber membrane layer obtained in step S8 is reinforced by a hot rolling mill to form a composite air filter material.
[0041] In this embodiment, the polylactic acid has a melting point of 145°C, a melt index of 30 g / 10 min, and a molecular weight of 7×10 4 , density is 1.25g / cm 3 .
[0042] Example 2
[0043] The other conditions are the same as those in Example 1, except that the quantitative amount of the nanofiber membrane layer in step S8 is 1 g / m 2 .
[0044] Example 3
[0045] The other conditions are the same as those in Example 1, except that the weight of the nanofiber membrane layer in step S8 is 5 g / m 2 .
[0046] Control group 1
[0047] Other conditions are the same as those in Example 1, except that step S1 is omitted and the biodegradable raw material used in step S2 is unmodified polylactic acid.
[0048] Control group 2
[0049] The other conditions are the same as those in Example 1, except that there is no step S2.
[0050] Control group 3
[0051] The other conditions are the same as those in Example 1, except that there is no step S6.
[0052] Control group 4
[0053] The other conditions are the same as those in Example 1, except that in step S6, only laser is used for etching.
[0054] Control group 5
[0055] The other conditions are the same as those in Example 1, except that in step S6, only the plasma beam is used for etching.
[0056] Control group 6
[0057] Other conditions are the same as those in Example 1, except that in step S6, the laser beam and the plasma beam are parallel.
[0058] Control group 7
[0059] The other conditions are the same as those in Example 1, except that in step S6, the laser beam and the plasma beam form an angle of 25°.
[0060] Control group 8
[0061] The other conditions are the same as those in Example 1, except that in step S6, the laser beam and the plasma beam form an angle of 50°.
[0062] The composite air filter materials prepared by the preparation methods of Examples 1 to 5 and Control Experiment Groups 1 to 8 were tested for filtration performance (filtration efficiency, initial resistance), moisture resistance (surface contact angle), temperature resistance (melting point) and strength performance (tensile strength). The test conditions are as follows:
[0063] Filtration efficiency: According to the test standard: EN143:2006;
[0064] Initial resistance: According to the test standard: EN143:2006;
[0065] Surface contact angle: According to the test standard: Tappi T 458 CM-2004;
[0066] Melting point: According to the test standard: ASTM D3954-15;
[0067] Tensile strength: According to the test standard: GB / T12914-2018.
[0068] The above performance test results are shown in Table 1.
[0069] Table 1 Performance test results
[0070]
[0071] From the results in Table 1, it can be seen that, by comparing Example 1, Example 2 and Example 3, the filtration efficiency of the composite filter material increases with the quantitative increase of the electrospun nanofiber membrane, but the initial resistance also increases accordingly.
[0072] By comparing Example 1 and Control Experiment Group 1, it can be seen that the tensile strength and melting point of Control Experiment Group 1 are significantly lower than those of Example 1, wherein the tensile strength reduction rate is close to 70%, which fully demonstrates that after the polylactic acid is modified in the present invention, the strength and temperature resistance of the molded composite air filter material are greatly improved.
[0073] By comparing Example 1 and Control Experiment Group 2, it can be seen that the tensile strength of Control Experiment Group 2 is lower than that of Example 1, indicating that the pretreatment in a low-temperature electric field of the present invention is beneficial to improving the strength of the formed composite air filter material.
[0074] By comparing Example 1 and Control Experiment Group 3, it can be seen that the surface contact angle of Control Experiment Group 3 is significantly lower than that of Example 1. The larger the surface contact angle, the better the hydrophobic performance. This proves that the present invention enhances the hydrophobicity of the fiber after using laser and plasma beam to adjust the surface microstructure of the fiber.
[0075] By comparing Example 1, Control Experiment Group 4 and Control Experiment Group 5, it can be seen that the surface contact angle of Example 1 is higher than those of Control Experiment Group 4 and Control Experiment Group 5, indicating that the present invention utilizes laser and plasma beams to simultaneously adjust the fiber surface microstructure, and its hydrophobic effect is better than that of using laser or plasma beams alone.
[0076] By comparing Example 1 and Control Experiment Group 6, it can be seen that the surface contact angle of Example 1 is higher than that of Control Experiment Group 6, indicating that the present invention is more conducive to tidying up the microstructure of the fiber surface after the laser and plasma beam are formed at a certain angle, so that it can obtain a better hydrophobic effect.
[0077] By comparing Example 1, Control Experiment Group 7 and Control Experiment Group 8, it can be seen that it is difficult to obtain a better hydrophobic etching effect when the angle between the laser and plasma beam is less than 30° or exceeds 45°.
[0078] In order to investigate the anti-ultraviolet performance of the composite air filter material prepared by the present invention, the composite air filter materials obtained in Example 1 and the control experimental group 1 were subjected to ultraviolet irradiation for 72 hours, and the change in tensile strength before and after irradiation was tested for evaluation. The anti-ultraviolet performance test results are shown in Table 2.
[0079] Table 2 UV resistance test results
[0080]
[0081] It can be seen from Table 2 that the composite air filter material prepared by modifying polylactic acid in the present invention greatly improves its anti-ultraviolet performance.
[0082] The embodiments of the present invention are described in detail above, but the contents are only preferred embodiments of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the present invention.
Claims
1. A method for preparing a composite air filter material, characterized in that: The following steps are involved: S1. Weigh 50 parts of polylactic acid chips, 5 parts of thiophenedicarboxylic acid, 5 parts of halogenated phenol, 3 parts of aromatic guanidine, 15 parts of palm kernel oil diethanolamide, 5 parts of maleic anhydride, and 3 parts of polyvinyl pyrrolidone by weight, mix and stir, then add 5 parts of tris(2,4-di-tert-butylphenyl)phosphite and 5 parts of 2-(2-hydroxy-5-methylphenyl)benzotriazole and stir to obtain modified polylactic acid; S2, pre-treating the modified polylactic acid in an electric field at -40°C and a voltage of 20 kV for 2 h; S3, drying the pretreated modified polylactic acid in vacuum; S4, heating the dried modified polylactic acid to form a melt; S5, the melt is extruded to form filaments, which are cooled and laid to form a fiber web, and the fiber web is hot-rolled to form a substrate; S6. The surface of the substrate fiber is etched and trimmed by using laser and plasma beams at the same time. The angle between the laser and plasma beams is 45°. The pulse energy of the laser is 5fs and the duration is 3min. The discharge power of the plasma beam is 300W. The voltage applied to the upper and lower positive and negative electrodes is 150V and the duration is 3min. The frequency of the excitation source is 40KHz. S7, dissolving the modified polylactic acid in a mixed solvent and stirring to dissolve to form a spinning solution, wherein the mixed solvent includes dioxane, acetone, dimethylformamide, dichloroethane and dichloromethane; the mass ratio of the dioxane, acetone, dimethylformamide, dichloroethane and dichloromethane is 10:30:20:10:20, and the spinning solution is formed by stirring and dissolving at 45° C.; the concentration of the spinning solution is 10%; S8, forming a nanofiber membrane layer with an average diameter of 0.7 μm on the substrate etched and trimmed in step S6 by electrostatic traction of the spinning solution, the electrostatic traction voltage is 20 kV, and the receiving distance is 20 cm; S9, forming a composite air filter material by hot rolling the substrate with the nanofiber membrane layer obtained in step S8.
2. The method for preparing the composite air filter material according to claim 1, characterized in that: In step S1, the polylactic acid chips, thiophenedicarboxylic acid, halogenated phenol, aromatic guanidine, palm kernel oil diethanolamide, maleic anhydride, and polyvinyl pyrrolidone are mixed and placed in a reaction kettle, stirred and reacted at a temperature of 20 to 30° C. for 1 to 3 hours, and tris(2,4-di-tert-butylphenyl)phosphite and 2-(2-hydroxy-5-methylphenyl)benzotriazole are added, and stirred and reacted at a temperature of 40 to 60° C. for 4 to 6 hours.
3. The method for preparing the composite air filter material according to claim 1, characterized in that: In step S3, the drying temperature is 80-90°C and the time is 6-10 hours.
4. The method for preparing the composite air filter material according to claim 1, characterized in that: In step S4, the heating temperature is set to 190-260°C.
5. The method for preparing the composite air filter material according to claim 1, characterized in that: In step S5, the melt is extruded to form filaments with a diameter of 4-6 μm, which are cooled by air and then formed into a fiber web on a web laying machine. The fiber web is reinforced by a hot rolling mill to form a substrate with a basis weight of 50-70 g / m 2 .
6. The method for preparing the composite air filter material according to claim 1, characterized in that: In step S8, the nanofiber membrane layer is quantitatively 1-5 g / m 2 .
Citation Information
Patent Citations
Ion production
GB1432006A
Method for improving surface hydrophilicity of transparent biological medical high polymer material
CN105254914A
Composite coating and preparation method thereof, silicone rubber protective sleeve and insulator
CN116426215A