A method for preparing nano-micron amorphous calcium carbonate using calcined corrugated paper as raw material and characterization thereof

The preparation of nano-micron-scale amorphous calcium carbonate by calcined corrugated cells solves the problems of insufficient utilization of shell resources and pollution of traditional processes, and achieves low-cost, environmentally friendly preparation processes and high-quality products, which are suitable for industrial applications.

CN118545743BActive Publication Date: 2024-11-19JIANGSU OCEAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410482890.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-22
Publication Date
2024-11-19
Estimated Expiration
2044-04-22

AI Technical Summary

Technical Problem

The existing technology fails to effectively utilize shell resources, resulting in the abandoned shells occupying the land and causing environmental pollution. The traditional calcium carbonate preparation process has problems of pollution and structural damage, which is difficult to meet the requirements of green, safety, ecological and environmental protection.

Method used

Using calcined corrugated tins as raw materials, nano-micron amorphous calcium carbonate is prepared through physical methods such as fuming, crushing, water extraction, and dialysis. Combined with Fourier infrared spectroscopy, XRD and scanning electron microscopy, the stability of the preparation process is ensured. and security.

Benefits of technology

It realizes low-cost, environmentally friendly nano-scale amorphous calcium carbonate preparation, avoids the use and pollution of chemical reagents, is suitable for industrial large-scale production, and ensures the quality and environmental friendliness of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118545743B_ABST
    Figure CN118545743B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing nanometer-level amorphous calcium carbonate using calcined corrugated paper as a raw material and a characterization method. The raw materials used in the method for preparing nanometer-level amorphous calcium carbonate components using calcined corrugated paper as a raw material are low in price and easy to obtain. The raw materials used in the invention are all calcium carbonate with a composition of more than 95% based on the calcined corrugated paper, which is relatively rich in content and suitable for popularization and use. The nanometer-level amorphous calcium carbonate components in the invention are prepared only by physical methods, which will neither change the shell structure nor cause pollution to the environment, is green and environmentally friendly, and has a simple preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of calcium carbonate preparation, and particularly relates to a method for preparing nano-micron-level amorphous calcium carbonate using calcined corrugated paper as a raw material and a characterization method. Background Art

[0002] Clam sphaerocephala Arca subcrenata Lischke, mud clams Arca granosa Linnaeus or Clam Arca inflata Reeve's shell. The records of the nature and taste of corrugated shell in the herbal books of all dynasties are mainly "warm, sweet, salty, and neutral", and the main treatment is "coldness in the heart and abdomen, coldness in the waist and spine, benefits the five internal organs, strengthens the stomach, and makes people eat". Nowadays, it is generally believed that corrugated shell is salty in taste, neutral in nature, can eliminate phlegm and resolve blood stasis, soften and disperse nodules, reduce acid and relieve pain, and can be used for stubborn phlegm, sticky and difficult to cough up, goiter, scrofula, lumps, stomach pain and acid reflux. Modern research shows that corrugated shell can promote the shrinkage of the liver and spleen, has a good effect on schistosomiasis liver and spleen enlargement, and is also used for other connective tissue hyperplasia lesions; it also has anti-cancer effects: modern clinical practice believes that it has a therapeutic effect on gastric cancer, intestinal cancer, and lung cancer, but its pharmacological effects are not yet fully understood.

[0003] At present, the utilization of shellfish resources in my country is basically limited to shellfish meat, and for calcium carbonate with a mass percentage of more than 80%, the utilization measures are not systematic and perfect. Therefore, with the rapid increase in shellfish production, the problem of the utilization of discarded shells has also emerged. These discarded shells are often dumped and piled up, which not only occupies land resources, but also often causes the breeding of mosquitoes and produces stench, which has great harm to the environment. The utilization of shells is one of the important factors restricting the development of the shellfish industry. As a natural biological resource, shells have a very high utilization value. If shell resources are fully utilized, not only can pollution and other problems be solved, but also the maximization of resource utilization and the virtuous cycle of production can be achieved, and the sustainable development of the shellfish industry can be promoted. Therefore, the utilization of shell resources needs to be solved urgently. Since shells are the exoskeletons of mollusks, the chemical composition of this type of traditional Chinese medicine has a common feature, that is, it contains about 95% calcium carbonate.

[0004] As an emerging biomedical raw material, the performance of calcium carbonate products affects and determines its functions and application range. Nano-micron amorphous calcium carbonate can release calcium ions in tumor tissue in response to the low pH microenvironment due to its special physical and chemical properties, induce tumor cell apoptosis through calcium ion overload, play an auxiliary anti-tumor role, and become a widely studied and applied calcium carbonate biomedical material. Therefore, the preparation of nano-micron amorphous calcium carbonate has always been a hot topic of research.

[0005] The purpose of the present invention is to provide a method for preparing nano-micron amorphous calcium carbonate components using calcined corrugated paper as raw materials and characterization thereof, and to provide a reference for ensuring that the nano-micron amorphous calcium carbonate components are stable, safe and controllable by determining the preparation process and its characterization method. Summary of the invention

[0006] The present invention proposes a method for preparing nano-micron-sized amorphous calcium carbonate using calcined corrugated paper as raw material and characterizing the method. The preparation method comprises taking an appropriate amount of discarded corrugated paper, crushing and sieving after calcining, adding appropriate purified water for soaking, reflux extraction twice, and filtering, dialysis, etc. to prepare a nano-micron-sized amorphous calcium carbonate component. The characterization method comprises using Fourier infrared spectroscopy to help detect the specific functional groups of the nano-micron-sized amorphous calcium carbonate component prepared using calcined corrugated paper as raw material, using XRD to determine the crystal form of the nano-micron-sized amorphous calcium carbonate component prepared using calcined corrugated paper as raw material, and using a scanning electron microscope to observe the specific morphology and size of the nano-micron-sized amorphous calcium carbonate component prepared using calcined corrugated paper as raw material. The product prepared by the present invention does not need to use some chemical reagents, has a simple production process, does not need to use precision equipment, and is environmentally friendly.

[0007] A method for preparing nano-micron amorphous calcium carbonate using calcined corrugated paper as raw material and characterizing the method, characterized in that the method is as follows:

[0008] S1: Raw material preparation: collect corrugated paper, soak it with purified water, remove the corrugated paper pulp, calcine it in a muffle furnace at 750°C for 0.5h, and crush it to obtain corrugated paper powder;

[0009] S2: Water extraction: Take the calcined corrugated shell powder, add 6 times the amount of water and soak for 30-60 minutes, heat in a heating jacket, reflux extraction for 45 minutes, and filter with filter paper; add 4 times the amount of water to the filter residue again, decoct for 30 minutes, and filter; combine the two filtrates; since shellfish drugs have a hard texture and a crisp texture after calcination, and soaking before decoction is conducive to the precipitation of active ingredients and increases the drug effect; relevant studies have shown that there is no significant difference in content between decoction twice and decoction three times, and the additional output does not match the cost and time invested, so the number of decoctions is determined to be twice;

[0010] S3: Concentration: The filtrate of S2 is filtered through a membrane, and the resulting liquid is concentrated under reduced pressure to a concentrate with a crude drug concentration of 5 g / mL;

[0011] S4: Pretreatment of dialysis bag: Take a dialysis bag of appropriate length and soak it in boiling water for 10 minutes. After the dialysis bag is softened, take it out and set it aside. The purpose of this step is to remove possible impurities and increase its permeability.

[0012] S5: Preparation of nano-micron-sized amorphous calcium carbonate components: Place the concentrated solution of S3 into a dialysis bag and dialyze for 72 hours, change the water every 4 hours, and store in a refrigerator at 4°C. The dialysis bag is a biological product with biological activity. Too high or too low temperature will cause it to lose its activity and have no dialysis effect. Frequent replacement of clean water can increase the concentration difference between the solutions inside and outside the dialysis bag and speed up the dialysis speed. After the dialysis is completed, evaporate the liquid in the dialysis bag to obtain the nano-micron-sized amorphous calcium carbonate components.

[0013] Furthermore, the corrugated metal in S1 is calcined corrugated metal, and the calcined corrugated metal powder is powder that passes through a 200-mesh sieve.

[0014] Furthermore, the water immersion temperature in S2 is 85-95° C., and the filtrate is obtained by using filter paper.

[0015] Furthermore, the filter membrane in S3 is a 0.22µm water filter membrane, the vacuum degree in the reduced pressure concentration is -0.1-0.08Mpa, and the temperature is 60°C.

[0016] Furthermore, the molecular cutoff of the dialysis bag is 1 KDa.

[0017] Furthermore, the functional groups, crystal forms and morphologies of the calcined corrugated powder are characterized.

[0018] Furthermore, the characterization of the functional groups of the calcined corrugated powder comprises the following steps:

[0019] The sample was passed through a 200-mesh sieve and dried at 60 °C for 3 h to constant weight. The sample was ground into flour and mixed evenly with potassium bromide (W / W, 1: 100) under an infrared drying lamp, and tableted at ≤ 10 Mpa. Potassium bromide was used as blank correction, and the Fourier transform infrared spectroscopy analysis conditions were 4 cm -1 Resolution, 16 scans accumulated, 4000-400 cm -1 The measurements were performed in the spectral range and each sample was measured twice in parallel.

[0020] Furthermore, the characterization of the calcined corrugated powder crystal type comprises the following steps:

[0021] The sample was ground and passed through a 200 mesh sieve. The X-ray tube used a copper target, Cu target Kα1 radiation, (λ=1.54Å), a slit of 0.5 mm, a test range angle: 5-90°; a scanning range angle: 20-80°, and a scanning speed of 10° / min.

[0022] Furthermore, the morphology characterization of the calcined corrugated powder comprises the following steps:

[0023] Step 1: Preparation

[0024] (1) Cut the sample to be observed into appropriate size and keep the surface as flat as possible;

[0025] (2) Clean the sample to remove any unnecessary dirt or dust;

[0026] Step 2: Sample processing

[0027] (3) If necessary, use sample pretreatment methods, such as metal evaporation or carbon coating, to improve the conductivity of the sample;

[0028] (4) Place the sample to be observed on the sample table and ensure that the sample is in good contact with the table surface;

[0029] Step 3: Vacuum treatment

[0030] (5) Place the sample stage into the sample chamber of the SEM;

[0031] (6) After closing the sample chamber, use a vacuum pump to extract the air in the chamber to ensure a vacuum environment in the sample chamber;

[0032] Step 4: Parameter settings

[0033] (7) Open the SEM software and connect to the SEM device;

[0034] (8) Set the acceleration voltage and magnification of the scanning electron microscope on the software interface and adjust them according to actual needs;

[0035] Step 5: Focus and Calibrate

[0036] (9) Focus the specimen in the electron microscope and adjust the objective and lens so that the image is clear;

[0037] (10) Perform necessary calibration, such as adjusting the scanning speed and scanning mode of the electron beam;

[0038] Step 6: Observe and photograph

[0039] (11) Click the "Start Scan" button on the software interface to start observing and photographing the sample;

[0040] (12) Use the zoom and navigation functions on the software interface to adjust the image details and position to obtain the desired observation results;

[0041] Step 7: Image analysis and saving

[0042] (13) Use the image analysis tools provided by the SEM software to analyze and measure the images, such as particle size distribution and surface morphology;

[0043] (14) After the analysis is completed, save the results to a computer for subsequent processing or reporting.

[0044] The following functions and effects can be obtained through the above technical solution:

[0045] The method for preparing nano-micron-level amorphous calcium carbonate components by using calcined corrugated paper as raw materials uses low-priced raw materials that are easily available.

[0046] The raw materials used in the present invention are all based on calcined corrugated board, the composition of which is more than 95% of calcium carbonate, which is rich in content and suitable for popularization and use.

[0047] The present invention adopts water as the extraction solvent to more comprehensively extract the nano-micron-level amorphous calcium carbonate components in the raw material. This study adopts reflux extraction, extracts twice, soaks for 30-60 minutes each time, and extracts for 45 minutes and 30 minutes respectively, with high efficiency and is very suitable for industrial-scale production. Studies have shown that the extraction efficiency is relatively highest when 6 times water and 4 times water are used respectively, extracted twice, soaked for 30-60 minutes each time, and extracted for 45 minutes and 30 minutes respectively.

[0048] The present invention adopts vacuum concentration, and a large number of experiments show that the vacuum concentration efficiency is high under this parameter. Vacuum concentration can increase the boiling point of the substance, thereby accelerating the concentration speed. The temperature of vacuum concentration is generally controlled between 40-80°C, and the specific temperature depends on the properties and stability of the extracted Chinese medicine components. Concentration generally takes a long time, and many effective components may decompose at 80°C; at 40°C, the temperature is too low, which will prolong the concentration time and increase energy consumption, so 60°C is generally selected. Using a 0.22µm water filter membrane, nano-micron-level amorphous calcium carbonate components with smaller particle size can be obtained. Dialysis is performed using a dialysis bag, and it is found that the dialysis efficiency of a 1KDa dialysis bag is generally the highest. Structural characterization is formulated based on the characteristics of calcium carbonate and based on certain basic research. Qualitative analysis is used to detect the quality of drugs, which saves time and effort, has a high accuracy rate, and can help identify the authenticity of drugs and ensure the uniformity, stability and reliability of drug quality. Structural characterization is of great significance for the accurate detection of nano- and micron-sized amorphous calcium carbonate components in corrugated paper, and is of great significance for the research, development and preparation of this drug and drugs in this field.

[0049] Structural characterization is a simple method for identifying calcium carbonate, which is easy to operate, has good reproducibility and high accuracy. In structural characterization, Fourier transform infrared spectroscopy is used to help detect the specific functional groups of nano-micron-scale amorphous calcium carbonate components prepared from calcined corrugated paper, which are generally OH-stretching vibration absorption peaks, CO3 2-The vibration peak of ions, etc.; XRD was used to determine the crystal form of nano-micron-scale amorphous calcium carbonate components prepared with calcined corrugated paper as raw material, which was mainly calcite-type calcium carbonate; scanning electron microscopy was used to observe the specific morphology and size of nano-micron-scale amorphous calcium carbonate components prepared with calcined corrugated paper as raw material, and the particle size was small, below 10µm. The scanning electron microscopy image after dialysis showed more pores, which may be due to the change in the crystal form of calcium oxide to form a large number of pores and a larger specific surface area; the experimental results were well expressed, with high accuracy, small error, and strong operability, and could make accurate qualitative analysis of nano-micron-scale amorphous calcium carbonate components prepared with calcined corrugated paper as raw material. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 This is Example 2, a method for preparing nano-micron-sized amorphous calcium carbonate components using calcined corrugated paper as raw material, characterized by Fourier infrared spectroscopy.

[0051] Figure 2 This is the X-ray spectral characterization of Example 2, a method for preparing nano-micron-sized amorphous calcium carbonate components using calcined corrugated paper as raw material.

[0052] Figure 3 This is a 2µm scanning electron microscope image of Example 2, a method for preparing nano-micron-sized amorphous calcium carbonate components using calcined corrugated paper as raw material.

[0053] Figure 4 This is a 10µm scanning electron microscope image of Example 2, a method for preparing nano-micron-sized amorphous calcium carbonate components using calcined corrugated paper as raw material. DETAILED DESCRIPTION

[0054] The following is combined with Figure 1-4 The present invention is further described as follows: Example

[0055] A method for preparing nano-micron-level amorphous calcium carbonate components using calcined corrugated paper as raw material comprises the following steps:

[0056] Step 1: Raw material preparation: collect corrugated paper from different origins, soak them in purified water, remove the corrugated paper pulp, dry them in a ventilated place, calcine them in a muffle furnace at 750°C for 0.5h, and crush them to obtain calcined corrugated paper powder;

[0057] Step 2: Water extraction: Take 100g of calcined corrugated bean powder, add 6 times the amount of water and soak for 30-60 minutes, heat in a heating jacket, reflux extract for 45 minutes, filter with filter paper; add 4 times the amount of water to the residue again, boil for 30 minutes, filter with filter paper. Combine the two filtrates.

[0058] Step 3: Concentration: The extract obtained in step 2 is filtered through a 0.22µm water filter membrane, and the resulting liquid is concentrated under reduced pressure to a concentrate having a crude drug concentration of 5g / mL;

[0059] Step 4: Pretreatment of dialysis bag: Take a dialysis bag of appropriate length and soak it in boiling water for 10 minutes. After the dialysis bag softens, take it out for use;

[0060] Step 5: Preparation of nano-micron-sized amorphous calcium carbonate components: Place the concentrated solution in a dialysis bag and dialyze for 72 hours, and store it in a refrigerator at 4°C; after the dialysis is completed, evaporate the liquid in the dialysis bag to dryness to obtain nano-micron-sized amorphous calcium carbonate components. Example

[0061] The characterization of the functional groups of calcined corrugated powder includes the following steps:

[0062] The sample was passed through a 200-mesh sieve and dried at 60 °C for 3 h to constant weight. The sample was ground into flour and mixed evenly with potassium bromide (W / W, 1: 100) under an infrared drying lamp, and tableted at ≤ 10 Mpa. Potassium bromide was used as blank correction, and the Fourier transform infrared spectroscopy analysis conditions were 4 cm -1 Resolution, 16 scans accumulated, 4000-400 cm -1 The measurements were performed in the spectral range and each sample was measured twice in parallel.

[0063] The characterization of the calcined corrugated powder crystal type includes the following steps:

[0064] The sample was ground and passed through a 200 mesh sieve. The X-ray tube used a copper target, Cu target Kα1 radiation, (λ=1.54Å), a slit of 0.5 mm, a test range angle: 5-90°; a scanning range angle: 20-80°, and a scanning speed of 10° / min.

[0065] The characterization of the morphology of calcined corrugated powder includes the following steps:

[0066] Step 1: Preparation

[0067] (1) Cut the sample to be observed into appropriate size and keep the surface as flat as possible.

[0068] (2) Clean the sample to remove any unnecessary dirt or dust.

[0069] Step 2: Sample processing

[0070] (3) If necessary, use sample pretreatment methods such as metal evaporation or carbon coating to improve the conductivity of the sample.

[0071] (4) Place the sample to be observed on the sample table, making sure that the sample is in good contact with the table surface.

[0072] Step 3: Vacuum treatment

[0073] (5) Place the sample stage into the sample chamber of the SEM.

[0074] (6) After closing the sample chamber, use a vacuum pump to extract the air in the chamber to ensure a vacuum environment in the sample chamber.

[0075] Step 4: Parameter settings

[0076] (7) Open the SEM software and connect to the SEM device.

[0077] (8) Set the acceleration voltage, magnification and other parameters of the scanning electron microscope on the software interface and adjust them according to actual needs.

[0078] Step 5: Focus and Calibrate

[0079] (9) Focus the specimen in the electron microscope and adjust the objective and lens so that the image is clear and visible.

[0080] (10) Perform necessary calibration, such as adjusting the scanning speed and scanning mode of the electron beam.

[0081] Step 6: Observe and photograph

[0082] (11) Click the "Start Scan" button on the software interface to begin observing and photographing the sample.

[0083] (12) Use the zoom and navigation functions on the software interface to adjust the image details and position to obtain the desired observation results.

[0084] Step 7: Image analysis and saving

[0085] (13) Use the image analysis tools provided by the SEM software to analyze and measure the images, such as particle size distribution and surface morphology.

[0086] (14) After the analysis is completed, save the results to a computer for subsequent processing or reporting.

[0087] The raw materials used in the method for preparing nano-micron-level amorphous calcium carbonate components using calcined corrugated paper as raw materials are cheap and easy to obtain; the raw materials used in the present invention are all based on calcium carbonate with a composition of more than 95% of calcined corrugated paper, which is relatively rich in content and suitable for promotion and use; the preparation of nano-micron-level amorphous calcium carbonate components in the present invention is only prepared by physical methods, and the traditional preparation of shell calcium carbonate components is generally prepared using acidic solutions or alkaline solutions, which will have the following problems, such as using organic reagents for extraction and soaking, and there is inevitable secondary pollution from acid treatment or alkali treatment, which is difficult to meet the green, safe, and ecological and environmentally friendly process requirements, and will destroy the original composition and structural structure of the shell. In this study, only some physical methods are used, which will neither change the shell structure nor pollute the environment, and are green and environmentally friendly, with a simple preparation process.

[0088] The above are all preferred embodiments of the present invention. For ordinary technicians in this technical field, without departing from the principle of the present invention, various equivalent modifications to the present invention belong to the protection scope of the claims attached to this application.

Claims

1. A method for preparing nano-micron amorphous calcium carbonate using calcined corrugated paper as raw material, characterized in that: The method is as follows: S1: Raw material preparation: collect corrugated paper, soak it with purified water, remove the corrugated paper meat, calcine it in a muffle furnace at 750°C for 0.5h, and crush it to obtain calcined corrugated paper powder; S2: Water extraction: Take the calcined corrugated powder, add 6 times the amount of water, soak for 30-60 minutes, heat in a heating mantle, reflux extraction for 45 minutes, filter with filter paper; add 4 times the amount of water to the residue again, boil for 30 minutes, filter; combine the two filtrates; S3: Concentration: The filtrate of S2 is filtered through a membrane, and the resulting liquid is concentrated under reduced pressure to a concentrate with a crude drug concentration of 5 g / mL; S4: Pretreatment of dialysis bag: Take a dialysis bag of appropriate length and soak it in boiling water for 10 minutes. After the dialysis bag is softened, take it out for use. The molecular retention capacity of the dialysis bag is 1KDa; S5: Preparation of nano-micron-sized amorphous calcium carbonate components: Place the concentrated solution of S3 into a dialysis bag and dialyze for 72 hours, and store it in a refrigerator at 4°C; after the dialysis is completed, evaporate the liquid in the dialysis bag to dryness to obtain nano-micron-sized amorphous calcium carbonate components.

2. The method for preparing nano-micron amorphous calcium carbonate using calcined corrugated paper as raw material according to claim 1, characterized in that: The calcined corrugated powder in S1 is powder that passes through a 200-mesh sieve.

3. The method for preparing nano-micron amorphous calcium carbonate using calcined corrugated paper as raw material according to claim 1, characterized in that: The water immersion temperature in S2 is 85-95°C, and the filtrate is obtained by using filter paper.

4. The method for preparing nano-micron amorphous calcium carbonate using calcined corrugated paper as raw material according to claim 1, characterized in that: The filter membrane in S3 is a 0.22µm water filter membrane, the vacuum degree in the reduced pressure concentration is -0.1-0.08Mpa, and the temperature is 60℃.