A processing technology for quartz special-shaped cold-processed parts and quartz special-shaped cold-processed parts
By cutting the part and plane grinding processes, the planarity and roughness of the support part of the quartz special-shaped cold-worked parts are improved, and combined with the combination of welding to fix the retaining part, the grinding difficulty and deformation problems are solved, and high-precision silicon wafer bearing and guide plate are achieved Effect.
Patent Information
- Application Number
- CN202410528372.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-04-29
AI Technical Summary
During the grinding process of quartz special-shaped cold-worked parts, the grinding of the upper surface of the support part is difficult to grind, resulting in poor plane quality. Subsequent pickling, flame polishing and annealing processing will cause deformation, further increasing the plane. degree tolerance.
The cutting part and plane grinding process are used to make the support part exposed and highlight, and then a single-sided grinder is used to grind the upper surface of the support part, and the retaining part and the support body are fixed by combining welding to ensure that the reference surface is coplanar. Improve installation accuracy and combined welding accuracy.
Improve the planarity and roughness quality of the support part, enhance the bearing capacity of the silicon wafer, reduce the disengagement of the silicon wafer, ensure high-precision coordination between the stopper and the support part, and improve the guide of the silicon wafer Accuracy and welding fixing effect.
Smart Images

Figure CN118545896B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of quartz part processing, and in particular to a processing technology for quartz special-shaped cold-processed parts and quartz special-shaped cold-processed parts. Background Art
[0002] Quartz glass products are widely used in many high-tech fields due to their excellent physical and chemical properties. They are resistant to high temperatures, have a small thermal expansion coefficient, good thermal stability, high purity, corrosion resistance, and good electrical insulation properties. Therefore, they occupy a very important position in the integrated circuit chip manufacturing industry, the photovoltaic solar energy manufacturing industry, and the LED solid lighting manufacturing industry, and have an irreplaceable position.
[0003] The quartz tray is an indispensable part in the silicon wafer transfer process. It is a quartz special-shaped cold-processed part, which includes a supporting body and a mounting part. The supporting body has an arc-shaped supporting part, and the silicon wafer is placed on the upper surface of the supporting part. The supporting body also has a stop part, which is higher than the supporting part. The stop part is used to horizontally limit the silicon wafer to prevent the silicon wafer from slipping out of the supporting part, and the mounting part is used to be installed and fixed with a manipulator. The manipulator is used to drive the quartz special-shaped cold-processed part and the silicon wafer to move together to place the silicon wafer into the positioning groove of the processing device. There are usually hundreds of positioning grooves, and the size of the positioning grooves is extremely small.
[0004] In order to reduce scratches on the silicon wafer, the upper surface of the support part needs to have good roughness. At the same time, the higher the matching accuracy between the silicon wafer and the quartz special-shaped cold-processed part, the less likely the silicon wafer will be bumped when placed in the positioning groove. Therefore, the upper surface of the support part needs to have a high flatness.
[0005] Therefore, during the preparation process of quartz special-shaped cold-processed parts, the upper surface of the supporting part needs to be ground to improve the roughness and flatness quality, and then pickled, flame polished and annealed in sequence to make the quartz round and translucent.
[0006] However, due to the existence of the stop part, the grinding of the upper surface of the supporting part is difficult and the grinding quality is poor. In addition, the subsequent pickling, flame polishing and annealing processes will cause certain deformation of the supporting part, further increasing the flatness tolerance. Summary of the Invention
[0007] In order to improve the flatness of the supporting surface, the present application provides a processing technology for a quartz special-shaped cold-worked part and a quartz special-shaped cold-worked part.
[0008] This application provides a process for processing special-shaped cold-worked quartz parts, which adopts the following technical solutions:
[0009] A process for processing special-shaped cold-worked quartz parts comprises the following steps:
[0010] S1. Milling molding: milling the quartz blank into a quartz milling part, the quartz milling part comprising a supporting body, a mounting portion and two front stop portions, the supporting body having a center hole, the upper surface of the supporting body protruding with an arc-shaped supporting portion, the supporting portion comprising two first supporting portions and a second supporting portion, the upper surfaces of the first supporting portion and the second supporting portion being coplanar, the curvature centers of the first supporting portion and the second supporting portion being both the axis of the center hole, the front stop portion being higher than the upper surface of the supporting portion, the inner concave side surface of the front stop portion being set as the first stop surface, the curvature center of the first stop surface being the axis of the center hole, and a first section to be cut being formed between the front stop portion and the first supporting portion; one side of the mounting portion is set as the rear stop portion, the rear stop portion is higher than the upper surface of the supporting portion, the inner concave side surface of the rear stop portion being set as the second stop surface, the curvature center of the second stop surface being the axis of the center hole, and a second section to be cut being formed between the rear stop portion and the second supporting portion;
[0011] S2. Grinding the reference surface: Grind the back of the quartz milling part. After grinding, the back is set as the reference surface. The bottom surfaces of the front stop, the supporting body and the mounting part are all reference surfaces.
[0012] S3. Cutting into parts: Cutting off the first to-be-cut section and the second to-be-cut section, so that the front stopper, the supporting body and the mounting part become independent units;
[0013] S4. Plane grinding: Grind the supporting body and the mounting part separately; use a single-sided grinder to grind the upper surface of the supporting part of the supporting body with the back of the supporting body as the reference surface; use a single-sided grinder to grind the upper surface of the mounting part with the back of the mounting part as the reference surface;
[0014] S5. Pickling: Pickling the front stopper, supporting body and mounting part;
[0015] S6. Flame polishing: flame polish the front stop, support body and mounting part;
[0016] S7. Combined welding: Clamp the front stop, the supporting body, and the mounting portion using a fixture, wherein the clamping reference plane is the reference plane common to the front stop, the supporting body, and the mounting portion; weld the cut surface of the front stop to the cut surface of the supporting body located on the first supporting portion side; and weld the cut surface of the rear stop to the cut surface of the supporting body located on the second supporting portion side.
[0017] S8. Annealing.
[0018] By adopting the above technical solution, by setting up cutting parts and plane grinding, the supporting part can be exposed and protruded, and then a single-sided grinder is used to grind the upper surface of the supporting part. The plane grinding method can greatly improve the flatness and roughness of the upper surface of the supporting part, so as to improve the bearing quality of the silicon wafer; finally, a combined welding method is adopted to weld and fix the front stop part and the rear stop part to the supporting body respectively, so that the front stop part and the rear stop part can limit the horizontality of the silicon wafer and reduce the occurrence of silicon wafer detachment.
[0019] In addition, the reference surface is ground to ensure that the reference surfaces of the front stopper, the supporting body and the mounting portion are coplanar, so as to facilitate subsequent processing and positioning, thereby ensuring the installation reference surface accuracy and combined welding accuracy of the mounting portion.
[0020] Optionally, in step S3, a cutting tool is used for cutting, and the widths of the first segment to be cut and the second segment to be cut are both larger than the size of the cutting tool; the cutting is performed three times, and in the first cutting, the center of curvature of the moving path of the cutting tool is the axis of the center hole, the curvature radius of the moving path of the cutting tool is set to R, and the size of the cutting tool is set to r. The cutting tool cuts off the first segment to be cut and the second segment to be cut, and the front stopper, the supporting body and the mounting part become independent entities; in the second cutting, the center of curvature of the moving path of the cutting tool is moved from the original center hole to the center hole. The center hole axis position is offset in the horizontal direction toward the first supporting part by a distance of two cutting tool sizes, and the curvature radius of the moving path of the cutting tool is Rr, so as to cut and trim the concave side surface of the front stop portion to form a cut surface; when cutting for the third time, the curvature center of the moving path of the cutting tool is adjusted, and the curvature center of the moving path of the cutting tool is offset in the horizontal direction toward the second supporting part by a distance of two cutting tool sizes from the center hole axis position, and the curvature radius of the moving path of the cutting tool is Rr, so as to cut and trim the concave side surface of the rear stop portion to form a cut surface.
[0021] By adopting the above technical solution, by setting the step-by-step cutting of the cutting tool, the center position of the curvature of the cutting path and the curvature radius of the cutting path, the curvature radius of the two pre-matched cutting surfaces are made consistent, so as to reduce the size of the cutting tool and cause the curvature radius of the two cutting surfaces to be inconsistent, thereby improving the matching accuracy of the two cutting surfaces, facilitating subsequent combined welding, thereby improving the matching accuracy between the stop part and the supporting part, and further improving the horizontal limiting effect of the stop part on the silicon wafer.
[0022] Optionally, in step S3, after the cut surface is formed, the lower edges of the cut surfaces of the front stop, the supporting body and the rear stop are chamfered; in step S7, during the clamping process, the cut surfaces of the front stop, the supporting body and the mounting part, the front stop, the supporting body and the rear stop are aligned and fitted together, the chamfers of adjacent cut surfaces are relatively arranged, the quartz welding wire is placed in the gap formed by the adjacent chamfers, and welding is performed using a welding gun.
[0023] By adopting the above technical solution, the matching and fitting of the two cut surfaces are first utilized to ensure the accuracy of the relative distance between the stop part and the supporting part. Secondly, a chamfer is set at the lower edge to accommodate solder, so as to facilitate the welding and fixation between the stop part and the supporting part, while also preventing the solder from overflowing to the fitting between the cut surfaces and affecting the matching accuracy of the cut surfaces.
[0024] Optionally, in step S3, after the chamfering is completed, a diamond notch is processed on the chamfered surface, and there are multiple diamond notches, which are arranged at intervals along the arc path of the cut surface, and the diamond notches extend through the chamfer; in step S7, a plurality of branch welding wires are extended from the outside of the quartz welding wire, and the branch welding wires are arranged at intervals along the length direction of the quartz welding wire. The quartz welding wire is located in the gap formed by adjacent chamfers, and the branch welding wire is located in the diamond notch.
[0025] By adopting the above technical solution and setting the diamond-shaped notch and the shape of the quartz welding wire, the contact areas between the solder and the blocking portion and the supporting portion are increased, thereby further improving the welding and fixing effect.
[0026] Optionally, in step S7, after the quartz welding wire is placed, the branch welding wires are first heated at intervals, and then different parts of the quartz welding wire are heated at intervals.
[0027] By adopting the above technical solution and arranging interval heating welding, the solder forming quality is improved.
[0028] Optionally, in step S7, the fixture includes a reference plate, a positioning frame is fixed on the lower surface of the reference plate, a negative pressure hole is provided in the reference plate, one end of the negative pressure hole passes through the lower surface of the reference plate, and an avoidance slot is passed through the upper surface of the reference plate; during the clamping process, the outer edges of the front stopper, the supporting body and the mounting part are constrained by the positioning frame, and the reference surfaces of the front stopper, the supporting body and the mounting part are attached to the lower surface of the reference plate, and the negative pressure of the negative pressure hole adsorbs and fixes the front stopper, the supporting body and the mounting part to the lower surface of the reference plate; the quartz welding wire is placed into the gap formed by adjacent chamfers through the avoidance slot.
[0029] By adopting the above technical solution and setting the specific structure of the fixture, the reference surfaces of the front stopper, the supporting body and the mounting part are fitted with the lower surface of the reference plate to improve the clamping and positioning effect, so that the reference surfaces of the front stopper, the supporting body and the mounting part are coplanar, thereby improving the combination accuracy, and by setting a positioning frame and negative pressure adsorption to improve the combination fixing progress, thereby improving the front stopper, the supporting body and the mounting part to maintain a high-precision combination during the welding process.
[0030] Secondly, by setting the avoidance slot, it is easy to put in the quartz welding wire and facilitate the heating and welding operation.
[0031] Optionally, in step S1, a plurality of strip grooves are milled on the back of the quartz milling part, and the strip grooves include a first groove and a second groove, wherein the first groove is located on the back of the supporting body, the second groove is located on the back of the mounting part, and the connecting position of the first groove and the second groove is located in the second section to be cut; in step S7, during the welding process, the first quartz tube is deployed, the first quartz tube is filled with inert gas, the middle part of the first quartz tube is bent, and the two ends of the first quartz tube are respectively pressed against the two ends of the strip groove, and the bent part of the first quartz tube is immersed in the molten solder, so that the bent part of the first quartz tube and the solder are cooled and solidified.
[0032] By adopting the above technical solution, when the quartz special-shaped cold-worked part carries a silicon wafer, the part of the quartz special-shaped cold-worked part away from the mounting part is more likely to bend downward under the action of its own weight and the gravity of the silicon wafer, and the first quartz tube filled with inert gas has greater elasticity and toughness. Therefore, the bent first quartz tube uses its own elasticity to resist the downward deformation tendency of the quartz special-shaped cold-worked part, thereby reducing the deviation of the silicon wafer and further improving the guide accuracy.
[0033] Moreover, when the quartz special-shaped cold-worked part sags too much due to vibration, the inner end wall of the first groove will press against the end of the first quartz tube to apply axial pressure to the first quartz tube, and the first quartz tube transfers the axial pressure to the inner end wall of the second groove, that is, the axial pressure is resisted by the more stable mounting portion, that is, the first quartz tube can also reduce the vibration sag of the quartz special-shaped cold-worked part, thereby reducing the damage or breakage of the welding portion between the supporting portion and the stop portion due to excessive sag.
[0034] Furthermore, the first quartz tube is in contact with the first quartz tube through molten solder, which is cooled and solidified to fix the first quartz tube in the strip groove, so as to reduce the falling off of the first quartz tube.
[0035] Optionally, step S9 is also included. After annealing, quartz powder is filled into the first groove and the second groove, the outer surface of the first quartz tube is set to a frosted surface, and the quartz powder covers the parts of the first quartz tube located in the first groove and the second groove, and the bent part of the first quartz tube is exposed. Then, an inorganic adhesive is sprayed at the notch position of the first groove and the second groove, and an inorganic adhesive is sprayed on the surface of the bent part of the first quartz tube. The inorganic adhesive penetrates into the surface of the quartz powder, so that the quartz powder at the notch of the first groove and the second groove is solidified to form a sealing part.
[0036] By adopting the above technical solution, by arranging quartz powder and a sealing portion, the quartz powder can contact the frosted surface of the first quartz tube. When the quartz special-shaped cold-worked part vibrates, the first quartz tube vibrates and slightly bends. The vibrating first quartz tube and the quartz powder undergo relative displacement, generating frictional heat, that is, converting the kinetic energy of the vibration into frictional heat energy, thereby playing a vibration-slowing role, thereby reducing the occurrence of damage or fracture of the welding part caused by high-frequency vibration.
[0037] Optionally, in step S1, an arcuate groove is milled on the back of the quartz milling part, the arcuate groove is connected to the strip groove, the depth of the arcuate groove is greater than the strip groove, the convex portion of the arcuate groove is arranged toward the center hole, the arcuate groove includes a first arcuate segment and two second arcuate segments, wherein the first arcuate segment is located on the lower surface of the supporting body, the two second arcuate segments are located on the lower surface of the mounting portion, and the connecting position between the first arcuate segment and the second arcuate segment is located at the second segment to be cut; in step S7 In the welding process, the second quartz tube is deployed first, and then the first quartz tube is deployed; the second quartz tube is arc-shaped, and the second quartz tube is filled with inert gas. The length of the second quartz tube is smaller than the length of the arc-shaped groove, and the curvature radius of the second quartz tube is larger than the curvature radius of the arc-shaped groove; when deploying the second quartz tube, the middle part of the second quartz tube is first elastically bent, and then the second quartz tube is placed in the arc-shaped groove, and a part of the second quartz tube is immersed in the molten solder, so that the part of the second quartz tube and the solder are cooled and solidified.
[0038] By adopting the above technical solution, when the quartz special-shaped cold-worked part bends downward when carrying a silicon wafer, the horizontally curved second quartz tube has a large bearing area between the supporting body and the mounting part, which can greatly resist the downward deformation tendency of the quartz special-shaped cold-worked part, thereby reducing the deviation of the silicon wafer and improving the guide accuracy.
[0039] Secondly, during the deployment of the second quartz tube, the second quartz tube is elastically bent so that the elastic force at both ends of the second quartz tube is applied to the side wall of the second arc segment away from the central axis of the quartz special-shaped cold-processed part, that is, the elastic force will be converted into a force that forces the supporting body and the mounting part to abut against each other, so as to resist the displacement trend of the supporting body from the mounting part due to the sagging deformation, thereby greatly improving the connection strength and positioning accuracy of the supporting body.
[0040] Furthermore, since the first quartz tube is deployed last, the first quartz tube will prevent the second quartz tube from escaping from the arc-shaped groove, thereby ensuring that the second quartz tube plays a role in strengthening the connection.
[0041] This application provides a special-shaped cold-worked quartz part, which adopts the following technical solution:
[0042] The invention discloses a quartz special-shaped cold-worked part, which is made by a quartz special-shaped cold-worked part processing technology.
[0043] In summary, this application includes at least one of the following beneficial technical effects:
[0044] 1. By setting up cutting parts, surface grinding and combined welding, the support part can be exposed and prominently set. Then, a single-side grinder is used to grind the upper surface of the support part. The surface grinding method can greatly improve the flatness and roughness of the upper surface of the support part, thereby improving the bearing quality of the silicon wafer;
[0045] 2. By setting the cutting tool's step-by-step cutting, the center position of the curvature of the cutting path, and the curvature radius of the cutting path, the curvature radius of the two pre-matched cutting surfaces is made consistent, thereby improving the matching accuracy of the two cutting surfaces, facilitating subsequent combined welding, thereby improving the matching accuracy between the stopper and the supporting part, and further improving the horizontal restraining effect of the stopper on the silicon wafer;
[0046] 3. By setting the specific structure of the fixture, the reference surfaces of the front stop, supporting body and mounting part are aligned with the lower surface of the reference plate to improve the clamping and positioning effect, so that the reference surfaces of the front stop, supporting body and mounting part are coplanar, thereby improving the assembly accuracy. In addition, by providing a positioning frame and negative pressure adsorption, the assembly fixing progress is accelerated, thereby improving the ability of the front stop, supporting body and mounting part to maintain a high degree of assembly accuracy during the welding process;
[0047] 4. When the quartz special-shaped cold-worked part carries a silicon wafer, the portion of the quartz special-shaped cold-worked part away from the mounting portion is more likely to bend downward under the action of its own weight and the gravity of the silicon wafer. The first quartz tube filled with inert gas has greater elasticity and toughness. Therefore, the curved first quartz tube uses its own elasticity to resist the sagging deformation tendency of the quartz special-shaped cold-worked part, thereby reducing the deviation of the silicon wafer and improving the guide accuracy. In addition, when the quartz special-shaped cold-worked part sags too much due to vibration, the inner end wall of the first groove will press against the end of the first quartz tube to apply axial pressure to the first quartz tube, and the first quartz tube will transfer the axial pressure to the inner end wall of the second groove, that is, the axial pressure is resisted by the more stable mounting portion.
[0048] 5. By providing quartz powder and a sealing portion, the quartz powder can contact the frosted surface of the first quartz tube. When the quartz special-shaped cold-worked part vibrates, the first quartz tube vibrates and slightly bends. The vibrating first quartz tube and the quartz powder undergo relative displacement, generating frictional heat. The kinetic energy of the vibration is converted into frictional heat, thereby playing a vibration-slowing role and reducing the possibility of damage or fracture of the welded parts caused by high-frequency vibration.
[0049] 6. When the quartz special-shaped cold-worked part carries the silicon wafer and bends downward, the horizontally curved second quartz tube has a large bearing area between the supporting body and the mounting portion, which can greatly resist the downward deformation tendency of the quartz special-shaped cold-worked part, thereby reducing the deviation of the silicon wafer and improving the guide accuracy; secondly, during the deployment of the second quartz tube, the second quartz tube is elastically bent, so that the elastic force at both ends of the second quartz tube is applied to the side wall of the second arc segment away from the central axis of the quartz special-shaped cold-worked part, that is, the elastic force will be converted into a force forcing the supporting body and the mounting portion to abut against each other, so as to resist the displacement tendency of the supporting body from the mounting portion due to the downward deformation, thereby greatly improving the connection strength and position accuracy of the supporting body. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 It is a schematic diagram of the overall structure of the special-shaped cold-worked quartz part of Example 1.
[0051] Figure 2 It is a top view of the quartz special-shaped cold-worked part of Example 1.
[0052] Figure 3 It is a flowchart of the processing technology of quartz special-shaped cold-worked parts in Example 1.
[0053] Figure 4 This is a schematic diagram of Example 1 for illustrating the changing process of cutting components.
[0054] Figure 5This is a schematic diagram of Example 2 for showing the back side of a special-shaped cold-worked quartz part.
[0055] Figure 6 It is a top view of the fixture of Example 2 clamping the quartz special-shaped cold-processed part.
[0056] Figure 7 yes Figure 6 Cross-sectional view in the AA direction.
[0057] Figure 8 This is a schematic diagram of Example 3 for showing the back side of a special-shaped cold-worked quartz part.
[0058] Figure 9 yes Figure 8 Cross-sectional view in the BB direction.
[0059] Figure 10 It is a partial cross-sectional view of Example 4 for demonstrating the covering relationship between the quartz powder and the first quartz tube.
[0060] Figure 11 This is a partial schematic diagram of Example 5 for showing the back side of a special-shaped cold-worked quartz part.
[0061] Explanation of the accompanying drawings: 1. supporting body; 2. mounting portion; 3. front stop portion; 6. first quartz tube; 7. strip groove; 8. arc-shaped strip groove; 9. second quartz tube; 10. center hole; 11. first supporting portion; 12. second supporting portion; 13. first section to be cut; 21. rear stop portion; 210. second stop surface; 22. second section to be cut; 23. chamfer; 24. diamond notch; 30. first stop surface; 51. reference plate; 52. avoidance slot; 53. positioning frame; 54. negative pressure hole; 61. quartz powder; 62. sealing portion; 71. first groove; 72. second groove; 81. first arc-shaped section; 82. second arc-shaped section. DETAILED DESCRIPTION
[0062] The following is combined with Figure 1-11 This application is described in further detail.
[0063] Example 1
[0064] Example 1 discloses a quartz special-shaped cold-worked part, such as Figure 1 、 Figure 2As shown, the quartz special-shaped cold-processed part includes a supporting body 1, a mounting portion 2 and two front stop portions 3. The supporting body 1 is a long strip structure. The supporting body 1 has a center hole 10. The upper surface of the supporting body 1 is protruded with an arc-shaped supporting portion. The supporting portion includes two first supporting portions 11 and one second supporting portion 12. The upper surfaces of the first supporting portion 11 and the second supporting portion 12 are coplanar. The centers of curvature of the first supporting portion 11 and the second supporting portion 12 are both the axis of the center hole 10. The upper surfaces of the first supporting portion 11 and the second supporting portion 12 are used to support silicon wafers.
[0065] The two front stop parts 3 are respectively arranged corresponding to the two first supporting parts 11, the front stop parts 3 are welded to the first supporting parts 11, the lower surface of the front stop part 3 is coplanar with the lower surface of the supporting body 1, the upper surface of the front stop part 3 is higher than the upper surface of the first supporting part 11, and the concave side surface of the front stop part 3 is set as the first stop surface 30. The center of curvature of the first stop surface 30 is the axis of the center hole 10, and the first stop surface 30 is used to limit the silicon wafer on the first supporting part 11.
[0066] The lower surface of the mounting portion 2 is coplanar with the lower surface of the supporting body 1, and a rear stop portion 21 is protruded from one side of the mounting portion 2 close to the supporting body 1. The rear stop portion 21 is welded to the second supporting portion 12, and the upper surface of the rear stop portion 21 is higher than the upper surface of the second supporting portion 12. The inner concave side surface of the rear stop portion 21 is set as a second stop surface 210, and the center of curvature of the second stop surface 210 is the axis of the center hole 10. The second stop surface 210 is used to limit the silicon wafer on the second supporting portion 12.
[0067] Example 1 also discloses the processing technology of the above-mentioned quartz special-shaped cold-worked parts, such as Figure 3 As shown, the following steps are included:
[0068] S1, milling molding: milling the quartz blank into quartz milling parts, such as Figure 4 As shown, during milling, a section to be cut is reserved. Specifically, a first section to be cut 13 is reserved between the front stop 3 and the first supporting portion 11 , and a second section to be cut 22 is reserved between the rear stop 21 and the second supporting portion 12 .
[0069] S2. Grinding the reference surface: Grind the back of the quartz milling part by surface grinding. After grinding, set the back of the quartz milling part as the reference surface. At this time, the bottom surfaces of the front stop 3, the supporting body 1 and the mounting part 2 are all reference surfaces.
[0070] S3, cutting the parts: cutting off the first to-be-cut segment 13 and the second to-be-cut segment 22, specifically, using a cutting tool to directly cut off the first to-be-cut segment 13 and the second to-be-cut segment 22, at this time, the center of curvature of the moving path of the cutting tool is the axis of the center hole 10, and the width of the first to-be-cut segment 13 and the second to-be-cut segment 22 is equal to the size of the cutting tool. This cutting method has high efficiency and good matching accuracy of the cut surface. After cutting, Figure 4 As shown, the front stopper 3, the supporting body 1 and the mounting portion 2 become independent entities.
[0071] S4. Plane grinding: Grind the supporting body 1 and the mounting portion 2 separately; use a single-side grinder to grind the upper surface of the supporting portion of the supporting body 1 with the back of the supporting body 1 as the reference surface.
[0072] The upper surface of the mounting portion 2 is ground using a single-side grinding machine with the back surface of the mounting portion 2 as a reference surface.
[0073] S5, pickling: pickling the front stopper 3, the supporting body 1 and the mounting portion 2.
[0074] S6. Flame polishing the front stopper 3, the supporting body 1 and the mounting portion 2.
[0075] S7. Combined welding: Use a fixture to clamp the front stopper 3, the supporting body 1 and the mounting part 2, wherein the reference surfaces for clamping are the bottom surfaces of the front stopper 3, the bottom surfaces of the supporting body 1 and the bottom surfaces of the mounting part 2; after clamping, a gap is reserved between the cut surface of the front stopper 3 and the cut surface of the supporting body 1 on the side of the first supporting part 11, and a gap is reserved between the cut surface of the rear stopper 21 and the cut surface of the supporting body 1 on the side of the second supporting part 12, and then a quartz welding wire is placed in the gap, and then a welding gun is used for heating and welding.
[0076] S8. Annealing.
[0077] The implementation principle of Example 1 is: by setting cutting parts and plane grinding, the supporting part can be exposed and protruded, and then a single-sided grinder is used to grind the upper surface of the supporting part. The plane grinding method can greatly improve the flatness and roughness of the upper surface of the supporting part, thereby improving the bearing quality of the silicon wafer.
[0078] Finally, the front stopper 3 and the rear stopper 21 are respectively welded and fixed to the supporting body 1 by a combined welding method, so that the front stopper 3 and the rear stopper 21 can limit the horizontality of the silicon wafer and reduce the occurrence of silicon wafer detachment.
[0079] Example 2
[0080] The difference between Example 2 and Example 1 is that Figure 5As shown, in step S3, cutting is performed three times, wherein the curvature radius of the moving path of the cutting tool is set to R, and the size of the cutting tool is set to r.
[0081] During the first cutting, the center of curvature of the moving path of the cutting tool is the axis of the center hole 10, and the cutting tool partially cuts off the first to-be-cut segment 13 and the second to-be-cut segment 22, so that the front stopper 3, the supporting body 1 and the mounting portion 2 become independent entities. During the second cutting, the center of curvature of the moving path of the cutting tool is offset from the original axis position of the center hole 10 toward the horizontal direction of the first supporting portion 11 by a distance of two cutting tool sizes, and the curvature radius of the moving path of the cutting tool is Rr, so as to cut the inner concave side of the front stopper 3. Cutting and trimming are performed to form a cut surface; when cutting for the third time, the curvature center of the moving path of the cutting tool is adjusted. The curvature center of the moving path of the cutting tool is the distance of two cutting tool sizes offset horizontally from the axial position of the center hole 10 toward the second supporting part 12. The curvature radius of the moving path of the cutting tool is Rr, so as to cut and trim the inner concave side surface of the rear stop part 21 to form a cut surface. Under this cutting method, the curvature radius of the cutting surface of the stop part and the cutting surface of the supporting part are consistent, so as to facilitate the subsequent high-precision combination and matching.
[0082] After the cut surface is formed, the lower edges of the cut surfaces of the front stop 3, the supporting body 1 and the rear stop 21 are chamfered 23. After the chamfer 23 is completed, the chamfer 23 surface is processed with a diamond notch 24. There are multiple diamond notches 24, and the diamond notches 24 are arranged at intervals along the arc path of the cut surface, and the diamond notches 24 pass through the chamfer 23.
[0083] In step S7, Figure 6 、 Figure 7 As shown, a non-standard fixture is selected for installation, which includes a reference plate 51, a positioning frame 53 is fixed to the lower surface of the reference plate 51, the inner side shape of the positioning frame 53 is consistent with the outer contour of the quartz special-shaped cold-processed part, a negative pressure hole 54 is provided in the reference plate 51, one end of the negative pressure hole 54 passes through the lower surface of the reference plate 51, and the other end of the negative pressure hole 54 is connected to the exhaust pipe, and the upper surface of the reference plate 51 is penetrated by a special-shaped avoidance slot 52.
[0084] During the clamping process, the front stop 3, the supporting body 1 and the mounting part 2 are placed in the positioning frame 53, and the outer edges of the front stop 3, the supporting body 1 and the mounting part 2 are constrained by the positioning frame 53, so that the cut surfaces of the front stop 3, the supporting body 1 and the rear stop 21 are aligned and fit together, and the chamfers 23 of adjacent cut surfaces are relatively arranged, and the reference surfaces of the front stop 3, the supporting body 1 and the mounting part 2 are all fit to the lower surface of the reference plate 51. At this time, the area within the avoidance slot 52 shows the reference surfaces of the front stop 3, the supporting body 1 and the mounting part 2, and the chamfer 23 of the cut surface is also displayed in the area of the avoidance slot 52.
[0085] Then the air is exhausted through the exhaust pipe, and the negative pressure generated by the negative pressure hole 54 adsorbs and fixes the front stopper 3 , the supporting body 1 and the mounting portion 2 on the lower surface of the reference plate 51 .
[0086] The quartz welding wire is placed into the gap formed by the adjacent chamfers 23 through the avoidance slot 52. In other embodiments, the existing quartz welding wire is selected. In this embodiment, the outer side of the quartz welding wire is extended to form a plurality of branch welding wires (not shown in the figure). The branch welding wires are arranged at intervals along the length direction of the quartz welding wire. The quartz welding wire is located in the gap formed by the adjacent chamfers 23. The branch welding wire is located in the diamond notch 24, and then welding is performed using a welding gun.
[0087] The welding order of the welding gun can be from top to bottom or from bottom to top, that is, step-by-step welding. The welding order of the welding gun can also be adjusted to improve the welding quality. Specifically, after placing the quartz welding wire, the welding gun first heats each branch welding wire at intervals. For example, after welding the first branch welding wire, the third and fifth branch welding wires are heated and welded, and then different parts of the quartz welding wire are heated at intervals.
[0088] Compared with the full welding method of the cut surface in Example 1, Example 2 first trims the cut surface to make the curvature radius of the two cut surfaces consistent, which can achieve a more perfect fitting effect, and then reserves space for solder accumulation by setting the chamfer 23 and the diamond notch 24, that is, the welding fixed position is located in a local position between the stop part and the supporting part, thereby reducing the occurrence of solder overflow or unstable welding gap due to full welding, which leads to a decrease in the fitting accuracy between the stop part and the supporting part. Furthermore, while ensuring high fitting accuracy, the stop part can accurately limit the movement of the silicon wafer, thereby reducing scratches caused by the offset and shaking of the silicon wafer.
[0089] Example 3
[0090] The difference between Example 3 and Example 2 is that Figure 8 、 Figure 9As shown, in step S1, a plurality of strip grooves 7 are milled on the back of the quartz milling part. In this embodiment, there are two strip grooves 7 symmetrically arranged along the central axis of the quartz milling part. The strip grooves 7 include a first groove 71 and a second groove 72, wherein the first groove 71 is located on the back of the supporting body 1, and the second groove 72 is located on the back of the mounting portion 2. The connecting position of the first groove 71 and the second groove 72 is located at the second segment to be cut 22.
[0091] In step S7, during the welding process, the first quartz tube 6 is deployed. The first quartz tube 6 is filled with an inert gas, preferably a high-pressure inert gas, so that the first quartz tube 6 has good elasticity and toughness. At the same time, the first quartz tube 6 is a curved tube with a curved middle portion.
[0092] During deployment, first ensure that the solder is in a molten state and the solder temperature is lower than the melting point of the first quartz tube 6. Then place the first quartz tube 6 into the strip groove 7 so that the two ends of the first quartz tube 6 are respectively pressed against the two ends of the strip groove 7, that is, part of the first quartz tube 6 is located in the first groove 71, and the other part is located in the second groove 72. The bent part of the first quartz tube 6 is immersed in the molten solder. After a period of time, the bent part of the first quartz tube 6 and the solder cool and solidify.
[0093] When the quartz special-shaped cold-worked part carries a silicon wafer, under the action of the weight of the supporting body 1 and the gravity of the silicon wafer, the supporting body 1 is more likely to bend downward relative to the mounting part 2, and the first quartz tube 6 uses its own elasticity to resist the downward deformation tendency of the quartz special-shaped cold-worked part, thereby reducing the deviation of the supporting body 1 and the silicon wafer, and thus improving the accuracy of the robot's wafer guide.
[0094] Moreover, when the manipulator drives the quartz special-shaped cold-worked part to move or guide the piece, if the supporting body 1 sags too much due to vibration, the inner end wall of the first groove 71 will press against the end of the first quartz tube 6 to apply axial pressure to the first quartz tube 6, and the first quartz tube 6 transfers the axial pressure to the inner end wall of the second groove 72, that is, the axial pressure is resisted by the more stable mounting portion 2, that is, the first quartz tube 6 can also reduce the vibration sag of the quartz special-shaped cold-worked part, thereby reducing the damage or breakage of the welding part between the supporting portion and the stop portion due to excessive sag.
[0095] Example 4
[0096] The difference between Example 4 and Example 3 is that Figure 10As shown, step S9 is also included, that is, after annealing, quartz powder 61 is filled in the first groove 71 and the second groove 72, and the outer surface of the first quartz tube 6 is set to a frosted surface. The quartz powder 61 covers the portion of the first quartz tube 6 located in the first groove 71 and the second groove 72, but does not cover the bent portion of the first quartz tube 6, so that the bent portion of the first quartz tube 6 is exposed, and the outer surface of the first quartz tube 6 is set to a frosted surface.
[0097] Then, an inorganic adhesive is sprayed on the notch positions of the first groove 71 and the second groove 72, and an inorganic adhesive is sprayed on the surface of the curved portion of the first quartz tube 6. At this time, the inorganic adhesive penetrates into the surface of the quartz powder 61. The surface area of the quartz powder 61 is large. The quartz powder 61 combines with the inorganic adhesive to form a relatively dense sealing portion 62. The sealing portion 62 is located at the notch positions of the first groove 71 and the second groove 72 to confine the remaining unpenetrated quartz powder 61 within the strip groove 7. The quartz powder 61 is in full contact with the frosted surface of the first quartz tube 6.
[0098] Therefore, when the quartz special-shaped cold-worked part vibrates, the first quartz tube 6 vibrates and slightly bends, and the vibrating first quartz tube 6 and the quartz powder 61 are relatively displaced, generating frictional heat, that is, converting the kinetic energy of vibration into frictional heat energy, thereby playing a role in vibration damping, so as to reduce the occurrence of damage or fracture of the welding part caused by high-frequency vibration.
[0099] Example 5
[0100] The difference between Example 5 and Example 3 is that Figure 11 As shown, in step S1, an arcuate groove 8 is milled on the back of the quartz milling part. The arcuate groove 8 is connected to the strip groove 7. The depth of the arcuate groove 8 is greater than that of the strip groove 7. The convex portion of the arcuate groove 8 is arranged toward the center hole 10. The arcuate groove 8 includes a first arcuate segment 81 and two second arcuate segments 82, wherein the first arcuate segment 81 is located on the lower surface of the supporting body 1, and the two second arcuate segments 82 are located on the lower surface of the mounting portion 2. The connecting position between the first arcuate segment 81 and the second arcuate segment 82 is located at the second segment to be cut 22.
[0101] In step S7, during the welding process, the second quartz tube 9 is deployed first, and then the first quartz tube 6 is deployed. Specifically, the second quartz tube 9 is arc-shaped and filled with an inert gas, preferably a high-pressure inert gas. The length of the second quartz tube 9 is smaller than the length of the arc-shaped groove 8. When no external force is applied, the curvature radius of the second quartz tube 9 is larger than the curvature radius of the arc-shaped groove 8.
[0102] When deploying the second quartz tube 9, the middle part of the second quartz tube 9 is first elastically bent so that the curvature radius of the elastically bent second quartz tube 9 is as consistent as possible with the regional radius of the arc-shaped groove 8, and then the second quartz tube 9 is placed in the arc-shaped groove 8. At this time, the middle part of the second quartz tube 9 is located in the first arc segment 81, and the two ends of the second quartz tube 9 are respectively located in the two second arc segments 82. After placement, the second quartz tube 9 recovers part of its deformation, and the end of the second quartz tube 9 elastically abuts against the side wall of the second arc segment 82 away from the central axis of the quartz special-shaped cold-worked part. At the same time, a part of the second quartz tube 9 is immersed in the molten solder. Finally, the first quartz tube 6 is deployed. The first quartz tube 6 can constrain the second quartz tube 9 in the arc-shaped groove 8 to prevent it from escaping.
[0103] The implementation principle of Example 5 is: when the quartz special-shaped cold-processed part carries a silicon wafer and bends downward, the horizontally curved second quartz tube 9 has a large bearing area between the supporting body 1 and the mounting portion 2, respectively, which can greatly resist the downward deformation tendency of the quartz special-shaped cold-processed part, thereby reducing the deviation of the silicon wafer and further improving the guide accuracy.
[0104] Secondly, the elastic force of the second quartz tube 9 is applied to the side wall of the second arc segment 82 away from the central axis of the quartz special-shaped cold-processed part, that is, the elastic force will be converted into a force that forces the supporting body 1 and the mounting part 2 to abut against each other, thereby resisting the displacement trend of the supporting body 1 from the mounting part 2 due to the sagging deformation, thereby greatly improving the connection strength and positioning accuracy of the supporting body 1.
[0105] The above are all preferred embodiments of the present application, and are not intended to limit the scope of protection of the present application. Therefore, any equivalent changes made based on the structure, shape, and principle of the present application should be included in the scope of protection of the present application.
Claims
1. A process for processing special-shaped cold-worked quartz parts, characterized in that: The following steps are involved: S1. Milling forming: The quartz blank is milled into a quartz milling part, wherein the quartz milling part comprises a supporting body (1), a mounting part (2) and two front stop parts (3), wherein the supporting body (1) has a center hole (10), and an arc-shaped supporting part is protruded from the upper surface of the supporting body (1), and the supporting part comprises two first supporting parts (11) and a second supporting part (12), wherein the upper surfaces of the first supporting part (11) and the second supporting part (12) are coplanar, and the curvature centers of the first supporting part (11) and the second supporting part (12) are both the axis of the center hole (10), and the front stop part (3) is higher than the upper surface of the supporting part. The concave side surface of the front stop portion (3) is set as a first stop surface (30), the center of curvature of the first stop surface (30) is the axis of the center hole (10), and a first section to be cut (13) is formed between the front stop portion (3) and the first supporting portion (11); one side of the mounting portion (2) is set as a rear stop portion (21), the rear stop portion (21) is higher than the upper surface of the supporting portion, the concave side surface of the rear stop portion (21) is set as a second stop surface (210), the center of curvature of the second stop surface (210) is the axis of the center hole (10), and a second section to be cut (22) is formed between the rear stop portion (21) and the second supporting portion (12); S2, grinding reference surface: grinding the back side of the quartz milling part. After grinding, the back side is set as the reference surface, and the bottom surfaces of the front stopper (3), the supporting body (1) and the mounting part (2) are all the reference surfaces; S3, cutting off the components: cutting off the first segment to be cut (13) and the second segment to be cut (22), so that the front stopper (3), the supporting body (1) and the mounting portion (2) become independent entities; S4, plane grinding: grinding the supporting body (1) and the mounting part (2) separately; using a single-sided grinding machine, with the back side of the supporting body (1) as a reference surface, grinding the upper surface of the supporting part of the supporting body (1); using a single-sided grinding machine, with the back side of the mounting part (2) as a reference surface, grinding the upper surface of the mounting part (2); S5, pickling: pickling the front stopper (3), the supporting body (1) and the mounting portion (2); S6, flame polishing: flame polishing the front stopper (3), the supporting body (1) and the mounting portion (2); S7, combined welding: using a fixture to clamp the front stopper (3), the supporting body (1) and the mounting part (2), wherein the clamping reference plane is a reference plane coplanar with the front stopper (3), the supporting body (1) and the mounting part (2); welding the cut surface of the front stopper (3) to the cut surface of the supporting body (1) located on the side of the first supporting part (11); welding the cut surface of the rear stopper (21) to the cut surface of the supporting body (1) located on the side of the second supporting part (12); S8. Annealing.
2. The process for processing special-shaped cold-worked quartz parts according to claim 1, characterized in that: In step S3, a cutting tool is used for cutting, wherein the widths of the first segment to be cut (13) and the second segment to be cut (22) are both greater than the size of the cutting tool; the cutting is performed in three steps, wherein during the first cutting, the center of curvature of the moving path of the cutting tool is the axis of the center hole (10), the radius of curvature of the moving path of the cutting tool is set to R, the size of the cutting tool is set to r, and the cutting tool cuts off the first segment to be cut (13) and the second segment to be cut (22), and the front stopper (3), the supporting body (1) and the mounting part (2) become independent entities; during the second cutting, the center of curvature of the moving path of the cutting tool is changed from the original The center hole (10) is offset horizontally toward the first supporting portion (11) at an axial position by a distance equal to two cutting tool sizes, and the radius of curvature of the moving path of the cutting tool is Rr, so as to cut and trim the concave side surface of the front stop portion (3) to form a cut surface; when cutting for the third time, the center of curvature of the moving path of the cutting tool is adjusted, and the center of curvature of the moving path of the cutting tool is offset horizontally toward the second supporting portion (12) at an axial position of the center hole (10) by a distance equal to two cutting tool sizes, and the radius of curvature of the moving path of the cutting tool is Rr, so as to cut and trim the concave side surface of the rear stop portion (21) to form a cut surface.
3. The process for processing special-shaped cold-worked quartz parts according to claim 1, characterized in that: In step S3, after the cut surfaces are formed, the lower edges of the cut surfaces of the front stopper (3), the supporting body (1) and the rear stopper (21) are chamfered (23); in step S7, during the clamping process, the cut surfaces of the front stopper (3), the supporting body (1) and the rear stopper (21) are aligned and fitted, the chamfers (23) of adjacent cut surfaces are arranged relative to each other, and the quartz welding wire is placed in the gap formed by the adjacent chamfers (23), and welding is performed using a welding gun.
4. The process for processing quartz special-shaped cold-worked parts according to claim 3 is characterized in that: In step S3, after the chamfer (23) is processed, a rhombus notch (24) is processed on the chamfer (23) surface, wherein there are a plurality of rhombus notches (24), the rhombus notches (24) are arranged at intervals along the arc path of the cut surface, and the rhombus notches (24) penetrate the chamfer (23); in step S7, a plurality of branch welding wires are extended from the outer side of the quartz welding wire, the branch welding wires are arranged at intervals along the length direction of the quartz welding wire, the quartz welding wires are located in the gap formed by adjacent chamfers (23), and the branch welding wires are located in the rhombus notches (24).
5. The process for processing quartz special-shaped cold-worked parts according to claim 4, characterized in that: In step S7, after the quartz welding wire is placed, the branch welding wires are first heated at intervals, and then different parts of the quartz welding wire are heated at intervals.
6. The process for processing quartz special-shaped cold-worked parts according to claim 4 or 5, characterized in that: In step S7, the fixture includes a reference plate (51), a positioning frame (53) is fixed on the lower surface of the reference plate (51), a negative pressure hole (54) is provided in the reference plate (51), one end of the negative pressure hole (54) penetrates to the lower surface of the reference plate (51), and an avoidance slot (52) is penetrated on the upper surface of the reference plate (51); during the clamping process, the outer edges of the front stopper (3), the supporting body (1) and the mounting part (2) are constrained by the positioning frame (53), the reference surfaces of the front stopper (3), the supporting body (1) and the mounting part (2) are in contact with the lower surface of the reference plate (51), and the negative pressure of the negative pressure hole (54) adsorbs and fixes the front stopper (3), the supporting body (1) and the mounting part (2) on the lower surface of the reference plate (51); and the quartz welding wire is placed in the gap formed by the adjacent chamfers (23) through the avoidance slot (52).
7. The process for processing quartz special-shaped cold-worked parts according to claim 3, characterized in that: In step S1, a plurality of strip grooves (7) are milled on the back of the quartz milling part, the strip grooves (7) comprising a first groove (71) and a second groove (72), wherein the first groove (71) is located on the back of the supporting body (1), the second groove (72) is located on the back of the mounting portion (2), and the connecting position of the first groove (71) and the second groove (72) is located at the second section to be cut (22); in step S7, during the welding process, the first quartz tube (6) is deployed, the first quartz tube (6) is filled with an inert gas, the middle part of the first quartz tube (6) is bent, the two ends of the first quartz tube (6) are respectively pressed against the two ends of the strip groove (7), and the bent part of the first quartz tube (6) is immersed in molten solder, so that the bent part of the first quartz tube (6) and the solder are cooled and solidified.
8. The process for processing special-shaped cold-worked quartz parts according to claim 7, characterized in that: The method further comprises step S9, wherein after annealing, quartz powder (61) is filled into the first groove (71) and the second groove (72), the outer surface of the first quartz tube (6) is set to be a frosted surface, the quartz powder (61) covers the portion of the first quartz tube (6) located in the first groove (71) and the second groove (72), and the bent portion of the first quartz tube (6) is exposed, and then an inorganic adhesive is sprayed at the notch position of the first groove (71) and the second groove (72), and the inorganic adhesive is sprayed on the surface of the bent portion of the first quartz tube (6), and the inorganic adhesive penetrates into the surface of the quartz powder (61), so that the quartz powder (61) at the notch position of the first groove (71) and the second groove (72) is solidified to form a sealing portion (62).
9. The process for processing special-shaped cold-worked quartz parts according to claim 7 or 8, characterized in that: In step S1, an arcuate groove (8) is milled on the back of the quartz milling part, the arcuate groove (8) is connected to the strip groove (7), the depth of the arcuate groove (8) is greater than that of the strip groove (7), the outer convex part of the arcuate groove (8) is arranged toward the central hole (10), and the arcuate groove (8) includes a first arcuate segment (81) and two second arcuate segments (82), wherein the first arcuate segment (81) is located on the lower surface of the supporting body (1), the two second arcuate segments (82) are located on the lower surface of the mounting portion (2), and the connecting position between the first arcuate segment (81) and the second arcuate segment (82) is located at the second segment to be cut (22 ); In step S7, during the welding process, the second quartz tube (9) is deployed first, and then the first quartz tube (6) is deployed; the second quartz tube (9) is arc-shaped, the second quartz tube (9) is filled with inert gas, the length of the second quartz tube (9) is less than the length of the arc-shaped strip groove (8), and the curvature radius of the second quartz tube (9) is greater than the curvature radius of the arc-shaped strip groove (8); when the second quartz tube (9) is deployed, the middle part of the second quartz tube (9) is first elastically bent, and then the second quartz tube (9) is placed in the arc-shaped strip groove (8), and a part of the second quartz tube (9) is immersed in the molten solder, so that the part of the second quartz tube (9) and the solder are cooled and solidified.
10. A quartz special-shaped cold-worked part, characterized in that: The product is made by the quartz special-shaped cold-worked parts processing technology described in claim 1.
Citation Information
Patent Citations
Epitaxial process quartz weldment and processing method thereof
CN110963686A
Square quartz boat and processing technology thereof
CN112234006A
Graphite boat for bearing silicon wafer and use method of graphite boat
CN115642122A
Single-silicon-chip loading device
CN204391066U
Half battery piece material box
CN216719893U