Ceramic brick and its preparation method and application

By replacing monovalent oxide flux in ceramic blanks and controlling chemical composition, the problem of taking into account both strength and whiteness of ceramic tiles is solved, and high whiteness, high intensity and micro-transmissive effects are achieved, suitable for Architectural decoration.

CN118545990BActive Publication Date: 2024-11-22GUANGDONG NEWPEARL CERAMIC GRP CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411027646.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-22
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

When existing ceramic wall and floor tiles increase the strength of the blank, the whiteness of the whiteness is easily reduced, resulting in the product being not beautiful enough and it is difficult to take into account both strength and whiteness, which affects the application range.

Method used

By replacing part of the monovalent oxide flux K2O and Na2O in the ceramic blank with dioxide flux MgO and CaO, and controlling its content, combining high-temperature melting and iron removal treatment, the glass phase is formed to improve transparency and whiteness. Maintain high intensity.

Benefits of technology

It realizes the high whiteness and high strength of the ceramic tile body, is suitable for rapid firing, has a slightly translucent effect, has a warm and delicate quality, and is suitable for architectural decoration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118545990B_ABST
    Figure CN118545990B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of building ceramic tiles, and specifically relates to a ceramic tile and a preparation method and application thereof. The ceramic tile of the present invention includes a ceramic body, wherein the ceramic body includes the following chemical components in weight percentage: Al2O3 18.56%~20.13%, SiO2 58.21%~61.34%, Fe2O3 0.05%~0.08%, TiO2 0.05%~0.10%, CaO 2.31%~3.65%, MgO 3.10%~4.65%, K2O 3.25%~4.25%, Na2O 2.15%~3.68%, and the rest are ignition loss and impurities. Under the joint action of various chemical components, the ceramic tile of the present invention not only has high strength and can be fired quickly, but also has high whiteness, and has a micro-transmittance effect at above 75°, and is suitable for building decoration, especially background wall decoration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building ceramic bricks, and in particular relates to a ceramic brick and a preparation method and application thereof. Background Art

[0002] At present, the production of ceramic wall and floor tiles is impacted by the market. Under the premise of increasingly weak profits, it is necessary to increase production to reduce costs, thereby improving the survival ability of enterprises. As the market demand for the size of ceramic wall and floor tiles increases, in order to ensure the yield rate, the requirements for the strength of the blank are getting higher and higher. Usually, when the strength of the blank is improved, the whiteness of the blank will decrease, resulting in the blank being dark and not beautiful enough. Especially with the application of rock slabs, the production of dining tables, bars and other products that require chamfering easily exposes the blank, resulting in the product blank being dark in whiteness, affecting its application effect, thereby affecting the application range of ceramic products. In the current existing technology, increasing the whiteness of the blank often requires washing and pickling the material for iron removal, and the plasticity of stone powder materials will decrease after washing or pickling, resulting in low strength of the formula blank. It can be seen that the existing product blanks are difficult to be compatible in terms of whiteness and strength. Therefore, it is necessary to develop a technology to solve this problem. Summary of the invention

[0003] In view of the problems existing in the prior art, the present invention aims to provide a ceramic tile and a preparation method and application thereof. The ceramic tile has a green body with both high whiteness and high strength and is suitable for production by a rapid sintering method.

[0004] Based on the above purpose, the technical solution adopted by the present invention is as follows:

[0005] In a first aspect, the present invention provides a ceramic tile, including a ceramic body, wherein the ceramic body includes the following chemical components in weight percentage: Al2O3 18.56%~20.13%, SiO2 58.21%~61.34%, Fe2O3 0.05%~0.08%, TiO2 0.05%~0.10%, CaO 2.31%~3.65%, MgO 3.10%~4.65%, K2O 3.25%~4.25%, Na2O 2.15%~3.68%, and the rest are loss on ignition and impurities.

[0006] The ceramic body of the ceramic tile adopts dioxide flux MgO and CaO to replace part of the monovalent oxide flux K2O and Na2O, and controls the contents of MgO, CaO, K2O and Na2O within the above-mentioned specific range, which not only enables rapid sintering, but also avoids the problem of dark whiteness of the body caused by only using monovalent oxide flux. Among them, MgO not only has a high-temperature fluxing effect, but also can promote the formation of a glass phase in the body. With the reasonable combination of the above-mentioned dioxide flux and monovalent oxide flux, under the joint action, the glass phase content is appropriate and evenly distributed, thereby increasing the transparency of the body and having a slightly light-transmitting effect. In addition, the iron content of the ceramic body is low, which reduces the negative impact of the iron element on the whiteness of the body.

[0007] The ceramic body of the ceramic tile has high strength, is suitable for a rapid firing production method, is not easy to break during the rapid firing process, and has a high yield rate; after firing, the whiteness is above 75°, has a slightly translucent effect, and has a warm and delicate texture, just like jade.

[0008] Preferably, the ceramic body comprises the following chemical components in weight percentage: Al2O3 19.05% to 19.65%, SiO2 59.24% to 60.87%, Fe2O3 0.06% to 0.07%, TiO2 0.06% to 0.08%, CaO 2.69% to 3.55%, MgO 3.68% to 4.05%, K2O 3.55% to 4.05%, Na2O 2.65% to 3.14%, and the rest is loss on ignition and impurities. When the ceramic body comprises the above-mentioned specific content of chemical components, it has better whiteness, light transmittance and green strength.

[0009] Preferably, the raw materials for preparing the ceramic green body include the following components in parts by weight: 6 to 10 parts of washed ball clay, 20 to 28 parts of washed potassium sodium stone powder, 3 to 5 parts of burned talc, 2 to 4 parts of diopside, 14.5 to 25.5 parts of calcined coal gangue, 15 to 25 parts of water-ground sodium stone powder, 10 to 16 parts of ultra-white sand, 2 to 4 parts of high-white bentonite, and 3 to 7 parts of wollastonite, wherein the ultra-white sand has a whiteness of more than 85° after firing, and the high-white bentonite has a whiteness of more than 75° after firing.

[0010] Washed ball clay contains the following chemical components in weight percentage: Al2O335.26%~40.25%, SiO257.24%~62.34%, TiO2≤0.15%, Fe2O3≤0.08%, and the rest is reduced as appropriate; it mainly provides Al2O3 and SiO2 components for the body, and mainly plays a skeleton role. Because the sand in the material is removed by water washing, it has higher whiteness and plasticity. The whiteness after firing is above 80°, such as 80°, 83° or the range formed by any two of the above values.

[0011] The washed potassium-sodium stone powder contains the following chemical components in percentage by weight: Al2O3 14.56%~18.90%, SiO2 61.34%~65.84%, K2O 6.35%~8.56%, Na2O 4.56%~6.98%, TiO2 0.05%~0.12%, Fe2O3≤0.08%; it mainly provides monovalent oxide flux components K2O and Na2O for the green body, plays a role in fluxing, can reduce the firing temperature, and increase the firing speed. Because it has been washed and iron-removed, the iron content in the material is greatly reduced, and the whiteness after firing is improved. The whiteness after firing is above 60°, such as 60°, 62° or the range formed by any two of the above values.

[0012] The burned talc contains the following chemical components in weight percentage: MgO 35.45%~38.69%, SiO2 61.04%~64.08%, and the rest are impurities; it mainly provides MgO for the green body, and the whiteness after burning is above 70°, such as 70°, 73°, 75° or the range formed by any two of the above values.

[0013] Diopside contains the following chemical components in weight percentage: Al2O3 15.78%~17.45%, SiO2 65.32%~68.69%, MgO 6.34%~8.56%, CaO 5.38%~7.69%, TiO2 0.10%~0.15%, Fe2O3 0.03%~0.05%; it mainly provides MgO and CaO for the body and has high-temperature fluxing properties. Compared with monovalent oxides, these divalent oxides can reduce the firing temperature without significantly reducing the whiteness of the body. After firing, the whiteness of diopside is above 45°, such as 45°, 47° or the range formed by any two of the above values.

[0014] Calcined gangue contains the following chemical components in weight percentage: Al2O3 44.35~46.53%, SiO2 52.14~54.44%, TiO2 0.03~0.06%, Fe2O≤0.08%; it mainly provides SiO2 and Al2O3 for the green body, and is the main substance for the green body to form mullite crystal phase and improve strength; coal gangue contains a large amount of carbon element, and during the calcination process, the carbon element has a strong reducing effect, and the iron element compounds in the coal gangue are reduced to form free iron that is easily adsorbed by a magnet. This method can greatly improve the whiteness of the material. The calcined gangue is used as the main material in the green body to improve the whiteness of the green body. After calcining, the whiteness of the calcined gangue is above 75°, such as 75°, 78°, 80° or the range formed by any two of the above values.

[0015] Water-ground sodium stone powder contains the following chemical components in weight percentage: Al2O3 14.56%~18.65%, SiO2 69.58%~73.24%, Na2O 8.64%~10.23%, K2O 1.23%~2.35%, TiO2 0.11%~0.15%, Fe2O3 0.05%~0.10%; it mainly provides monovalent oxide Na2O component for the blank, which plays a role of flux. This material is formed into fine particles through water grinding, and then iron removal is carried out to remove most of the iron in the material, thereby ensuring the whiteness of the material. The whiteness of the water-ground sodium stone powder after firing is above 45°, such as the range formed by any two values ​​above 45° and 48°.

[0016] Super white sand contains the following chemical components in weight percentage: Al2O3 10.24%~14.35%, SiO2 84.21%~87.64%, K2O 0.5%~0.8%, Na2O 1.24%~2.54%, TiO2 0.12%~0.15%, Fe2O3 0.08%~0.11%; it provides the main skeleton component for the green body, and its iron content is relatively low, which can greatly improve the whiteness of the green body. The whiteness of super white sand after firing is above 85°, such as 85°, 87° or the range formed by any two of the above values.

[0017] High white bentonite contains the following chemical components in weight percentage: Al2O330.21%~33.54%, SiO263.54%~66.58%, TiO20.12%~0.21%, Fe2O30.09~0.12%; it provides the main skeleton components for the green body. At the same time, in addition to having higher viscosity, high white bentonite can greatly improve the strength of the green body and improve the whiteness of the product compared to ordinary bentonite. The whiteness of high white bentonite after firing is above 75°, such as the range formed by any two values ​​above 75° and 78°.

[0018] Wollastonite contains the following chemical components in weight percentage: CaO 47.25%~49.25%, SiO2 50.65%~52.65%; it mainly provides the solvent CaO and the main skeleton components for the green body.

[0019] The main element that affects the whiteness of the blank is iron, which mainly exists in the form of free iron and compounds in the blank material. Free iron is relatively easy to remove, while iron in the form of compounds is difficult to remove, which is the main factor affecting the whiteness of the blank. The ceramic blank adopts calcined coal gangue that is easy to remove iron after calcination as the main raw material, which greatly reduces the iron content of the blank. In addition, other materials selected have less iron content, so that the product has a higher whiteness after firing. At the same time, by matching divalent oxides and monovalent oxides in a reasonable proportion, the needs of rapid firing can be met, and the problem of dark whiteness of the blank caused by only using monovalent oxide flux can be avoided. At the same time, a glass phase can be formed and evenly distributed, so that the product blank has a micro-translucent effect. The ceramic blank made by the above raw material formula has a higher strength and is suitable for a rapid firing production method. After firing, the whiteness is above 75°, and it has a micro-translucent effect. The quality texture is warm and delicate, just like jade.

[0020] The whiteness of the washed ball clay, the washed potassium sodium stone powder, the burned talc, the diopside, the calcined coal gangue, the water-ground sodium stone powder, the ultra-white sand and the high-white bentonite after firing can be measured by the following method: The steps are as follows: 1. Add the raw materials into water and obtain a slurry by ball milling. The fineness of the slurry is 0.8~1.2wt.% on a 320-mesh sieve, and the moisture content is between 35.8~37.0wt.%. 2. The slurry is dried and powdered, and a cylindrical cake-shaped material with a diameter of 6cm and a thickness of 0.8cm is pressed. 3. Fire in a kiln at 1180° for 65 minutes. 4. After cooling, use a digital whiteness meter to directly measure the whiteness, which can directly display the above-mentioned whiteness data.

[0021] Preferably, among the raw materials for preparing the ceramic green body, washed ball clay is 7 to 8 parts by weight, washed potassium sodium stone powder is 23 to 25 parts by weight, calcined coal gangue is 17.5 to 22.5 parts by weight, water-ground sodium stone powder is 18 to 22 parts by weight, and super white sand is 12 to 14 parts by weight. When the washed ball clay, washed potassium sodium stone powder, calcined coal gangue, water-ground sodium stone powder and super white sand are within the above-mentioned specific dosage range, the obtained ceramic body includes the following chemical components in weight percentage: Al2O3 19.05%~19.65%, SiO2 59.24%~60.87%, Fe2O3 0.06%~0.07%, TiO2 0.06%~0.08%, CaO 2.69%~3.55%, MgO 3.68%~4.05%, K2O 3.55%~4.05%, Na2O 2.65%~3.14%, and the rest are loss on ignition and impurities, and the rest are loss on ignition and impurities, and have better whiteness, transmittance and green strength.

[0022] Preferably, the ceramic tile further comprises a glaze layer and a pattern layer; the ceramic body, the glaze layer and the pattern layer are stacked in sequence;

[0023] 49.88%~52.14%, K2O: 2.34%~3.65%, Na2O: 2.31%~3.68%, CaO: 3.65%~5.34%, M gO: 1.24%~2.35%, BaO: 2.34%~5.32%, ZnO: 2.31%~4.21%, ZrO2: 6.31%~8.25%.

[0024] Preferably, the whiteness of the ceramic body is above 75°, such as 75°, 76°, 77°, 78°, 79°, 80° or a range formed by any two of the above values.

[0025] In a second aspect, the present invention provides a method for preparing the ceramic tile, comprising the following steps:

[0026] Washed ball clay, washed potassium sodium stone powder, burned talc, diopside, calcined coal gangue, water-ground sodium stone powder, super white sand, high white bentonite and wollastonite are mixed, and then water, a water reducing agent and a suspending agent are added, and ball milling is performed to obtain a green body slurry;

[0027] The obtained green body slurry is subjected to iron removal and spray drying to obtain green body powder;

[0028] The obtained green body powder is pressed into shape and dried to obtain a dry brick;

[0029] The obtained dried bricks are glazed, patterned and fired to obtain ceramic tiles.

[0030] Preferably, in the process of preparing the green body slurry, based on the total weight of the washed ball clay, the washed potassium sodium stone powder, the burned talc, the diopside, the calcined coal gangue, the water-ground sodium stone powder, the ultra-white sand, the high white bentonite and the wollastonite, the weight of the water is 38% to 42%, the weight of the water reducer is 0.25% to 0.35%, and the weight of the suspending agent is 0.15% to 0.20%.

[0031] Preferably, the water reducing agent comprises sodium tripolyphosphate.

[0032] Preferably, the suspending agent comprises sodium methylcellulose.

[0033] Preferably, the moisture content of the green body powder is 6.5wt.%~7.0wt.%.

[0034] Preferably, the strength of the dried brick is 1.8-2.4 MPa.

[0035] Preferably, the sintering temperature is 1185°~1195°C, and the sintering time is 60~70 minutes.

[0036] In a third aspect, the present invention further provides the application of the ceramic tile in architectural decoration. The ceramic tile has a micro-light-transmitting effect, especially when applied to a background wall area, it has a hazy light-transmitting effect.

[0037] In a fourth aspect, the present invention further provides application of the ceramic tile in background wall decoration.

[0038] Compared with the prior art, the beneficial effects of the present invention are as follows: under the joint action of various chemical components, the ceramic body of the ceramic tile of the present invention not only has high strength and can be fired quickly, is not easy to break during the rapid firing process, has a high yield, but also has high whiteness, above 75°, and has a slightly light-transmitting effect, and is suitable for architectural decoration, especially background wall decoration. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a photo of the light transmission effect of the front side of the ceramic tile in Example 1;

[0040] Figure 2 This is a photo of the light transmission effect of the back of the ceramic tile in Example 1;

[0041] Figure 3 This is a photo of the light transmission effect of the front side of the ceramic tile of comparative example 1. DETAILED DESCRIPTION

[0042] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0043] Unless otherwise specified, the test methods used in the examples are all conventional methods; the materials, reagents, etc. used, unless otherwise specified, can be obtained from commercial channels; the same raw materials have the same source.

[0044] Example 1

[0045] This embodiment provides a ceramic tile, and the preparation method thereof comprises the following steps:

[0046] (1) Calcine the gangue at 1200°C for 8 hours to reduce the iron compounds to form free iron by the carbon element in the gangue, and then use iron removal equipment to remove iron to obtain 78° calcined gangue;

[0047] (2) Mix the following raw materials in parts by weight to obtain a mixed raw material for a ceramic body: 8 parts of washed ball clay, 24 parts of washed sodium potassium stone powder, 4 parts of calcined talc, 3 parts of diopside, 20 parts of calcined coal gangue obtained in step (1), 20 parts of water-ground sodium stone powder, 13 parts of ultra-white sand, 3 parts of high-white bentonite, and 5 parts of wollastonite;

[0048] (3) adding 42% by total weight of water, 0.35% by weight of sodium tripolyphosphate and 0.15% by weight of sodium methylcellulose to the mixed raw materials of the ceramic green body obtained in step (2), and ball milling to obtain a green body slurry having a water content of 36.5%;

[0049] (4) removing iron from the green body slurry obtained in step (3) using an iron removal device and spray drying to obtain a green body powder having a moisture content of 6.5 wt.%;

[0050] (5) The green body powder obtained in step (4) is pressed into a brick of required specifications by a press, and then dried to obtain a dried brick;

[0051] (6) The dried brick obtained in step (5) is glazed and patterned by a glaze line, and then fired at a temperature of 1188° C. for 62 min to obtain a ceramic brick.

[0052] The ceramic tile obtained in this embodiment contains the following chemical components in percentage by weight: Al2O3 19.34%, SiO2 59.77%, Fe2O3 0.06%, TiO2 0.07%, CaO 2.98%, MgO 3.87%, K2O 3.75%, Na2O 2.91%, and the rest are reduced materials and impurities.

[0053] The glaze in the ceramic tile obtained in this embodiment contains the following chemical components in weight percentage: Al2O3: 22.29%, SiO2: 51.01%, K2O: 2.99%, Na2O: 2.99%, CaO: 4.49%, MgO: 1.79%, BaO: 3.83%, ZnO: 3.26%, and ZrO2: 7.28%.

[0054] Example 2

[0055] This embodiment provides a ceramic tile, and its preparation method is different from that of embodiment 1 in that the water-washed potassium sodium stone powder used in step (2) is 20 parts by weight. The green body of the ceramic tile obtained in this embodiment contains the following chemical components in percentage by weight: Al2O3 19.04%, SiO2 60.77%, Fe2O3 0.07%, TiO2 0.08%, CaO 2.86%, MgO 3.89%, K2O 3.35%, Na2O 2.41%, and the rest are reduced and impurities.

[0056] Example 3

[0057] This embodiment provides a ceramic tile, and its preparation method is different from that of embodiment 1 in that the water-washed potassium sodium stone powder used in step (2) is 28 parts by weight. The green body of the ceramic tile obtained in this embodiment contains the following chemical components in percentage by weight: Al2O3 19.66%, SiO2 60.77%, Fe2O3 0.08%, TiO2 0.06%, CaO 2.79%, MgO 3.67%, K2O 4.25%, Na2O 3.68%, and the rest are reduced and impurities.

[0058] Example 4

[0059] This embodiment provides a ceramic tile, and its preparation method is different from that of embodiment 1 in that the amount of calcined talc used in step (2) is 3 parts by weight. The green body of the ceramic tile obtained in this embodiment contains the following chemical components in percentage by weight: Al2O3 19.64%, SiO2 59.81%, Fe2O3 0.07%, TiO2 0.08%, CaO 2.88%, MgO 3.10%, K2O 3.65%, Na2O 2.87%, and the rest are reduced and impurities.

[0060] Example 5

[0061] This embodiment provides a ceramic tile, and its preparation method is different from that of embodiment 1 in that the amount of calcined talc used in step (2) is 5 parts by weight. The green body of the ceramic tile obtained in this embodiment contains the following chemical components in percentage by weight: Al2O3 18.64%, SiO2 58.81%, Fe2O3 0.08%, TiO2 0.08%, CaO 2.68%, MgO 4.65%, K2O 3.90%, Na2O 2.79%, and the rest are reduced and impurities.

[0062] Example 6

[0063] This embodiment provides a ceramic tile, and its preparation method is different from that of embodiment 1 in that the calcined coal gangue used in step (2) is 15 parts by weight. The green body of the ceramic tile obtained in this embodiment contains the following chemical components in percentage by weight: Al2O3 19.04%, SiO2 58.41%, Fe2O3 0.08%, TiO2 0.08%, CaO 3.18%, MgO 3.18%, K2O 3.95%, Na2O 3.09%, and the rest are reduced and impurities.

[0064] Example 7

[0065] This embodiment provides a ceramic tile, and its preparation method is different from that of embodiment 1 in that the calcined coal gangue used in step (2) is 25 parts by weight. The green body of the ceramic tile obtained in this embodiment contains the following chemical components in percentage by weight: Al2O3 20.12%, SiO2 60.81%, Fe2O3 0.08%, TiO2 0.06%, CaO 2.88%, MgO 3.15%, K2O 3.65%, Na2O 2.71%, and the rest are reduced and impurities.

[0066] Example 8

[0067] The present embodiment provides a ceramic tile, and the preparation method thereof is different from that of the embodiment 1 in that the mixed raw materials for the ceramic body are obtained according to the following raw material formula in parts by weight in step (2): 6 parts of washed ball clay, 20 parts of washed sodium potassium stone powder, 4 parts of calcined talc, 3 parts of diopside, 25 parts of calcined coal gangue obtained in step (1), 15 parts of water-ground sodium stone powder, 10 parts of ultra-white sand, 3 parts of high-white bentonite, and 5 parts of wollastonite. The ceramic tile obtained in the present embodiment contains the following chemical components in weight percentage: Al2O3 18.58%, SiO2 61.24%, Fe2O3 0.07%, TiO2 0.09%, CaO 3.57%, MgO 3.88%, K2O 3.98%, Na2O 2.68%, and the rest are reduced and impurities.

[0068] Example 9

[0069] The present embodiment provides a ceramic tile, and the preparation method thereof is different from that of the embodiment 1 in that the mixed raw materials for the ceramic body are obtained according to the following raw material formula in parts by weight in step (2): 7 parts of washed ball clay, 23 parts of washed sodium potassium stone powder, 4 parts of calcined talc, 3 parts of diopside, 22 parts of calcined coal gangue obtained in step (1), 18 parts of water-ground sodium stone powder, 12 parts of ultra-white sand, 3 parts of high-white bentonite, and 5 parts of wollastonite. The ceramic tile obtained in the present embodiment contains the following chemical components in weight percentage: Al2O3 19.08%, SiO2 60.55%, Fe2O3 0.06%, TiO2 0.07%, CaO 2.88%, MgO 3.85%, K2O 3.85%, Na2O 3.04%, and the rest are reduced and impurities.

[0070] Example 10

[0071] The present embodiment provides a ceramic tile, and the preparation method thereof is different from that of the embodiment 1 in that the mixed raw materials for the ceramic body are obtained according to the following raw material formula in parts by weight in step (2): 8 parts of washed ball clay, 25 parts of washed sodium potassium stone powder, 4 parts of calcined talc, 3 parts of diopside, 18 parts of calcined coal gangue obtained in step (1), 22 parts of water-ground sodium stone powder, 14 parts of ultra-white sand, 3 parts of high-white bentonite, and 5 parts of wollastonite. The ceramic tile obtained in the present embodiment contains the following chemical components in weight percentage: Al2O3 19.55%, SiO2 59.85%, Fe2O3 0.06%, TiO2 0.08%, CaO 3.45%, MgO 3.85%, K2O 4.00%, Na2O 3.08%, and the rest are reduced and impurities.

[0072] Embodiment 11

[0073] The present embodiment provides a ceramic tile, and the preparation method thereof is different from that of the embodiment 1 in that the mixed raw materials for the ceramic body are obtained according to the following raw material formula in parts by weight in step (2): 10 parts of water-washed ball clay, 28 parts of water-washed sodium potassium stone powder, 4 parts of calcined talc, 3 parts of diopside, 15 parts of calcined coal gangue obtained in step (1), 30 parts of water-ground sodium stone powder, 16 parts of ultra-white sand, 3 parts of high-white bentonite, and 5 parts of wollastonite. The ceramic tile obtained in the present embodiment contains the following chemical components in percentage by weight: Al2O3 20.01%, SiO2 58.33%, Fe2O3 0.06%, TiO2 0.08%, CaO 2.88%, MgO 3.19%, K2O 3.75%, Na2O 2.68%, and the rest are reduced and impurities.

[0074] Example 12

[0075] The present embodiment provides a ceramic tile, and the preparation method thereof is different from that of the embodiment 1 in that the mixed raw materials for the ceramic body are obtained according to the following raw material formula in parts by weight in step (2): 6 parts of washed ball clay, 20 parts of washed sodium potassium stone powder, 3 parts of calcined talc, 2 parts of diopside, 25 parts of calcined coal gangue obtained in step (1), 15 parts of water-ground sodium stone powder, 10 parts of ultra-white sand, 2 parts of high-white bentonite, and 3 parts of wollastonite. The ceramic tile obtained in the present embodiment contains the following chemical components in percentage by weight: Al2O3 18.66%, SiO2 61.32%, Fe2O3 0.06%, TiO2 0.08%, CaO 2.38%, MgO 3.11%, K2O 3.98%, Na2O 3.08%, and the rest are reduced and impurities.

[0076] The glaze in the ceramic tile obtained in this embodiment contains the following chemical components in weight percentage: Al2O3: 21.05%, SiO2: 51.91%, K2O: 2.89%, Na2O: 2.90%, CaO: 4.69%, MgO: 1.99%, BaO: 3.89%, ZnO: 3.29%, ZrO2: 7.38%.

[0077] Example 13

[0078] The present embodiment provides a ceramic tile, and the preparation method thereof is different from that of the embodiment 1 in that the mixed raw materials for the ceramic body are obtained according to the following raw material formula in parts by weight in step (2): 10 parts of washed ball clay, 28 parts of washed sodium potassium stone powder, 5 parts of calcined talc, 4 parts of diopside, 15 parts of calcined coal gangue obtained in step (1), 30 parts of water-ground sodium stone powder, 16 parts of ultra-white sand, 4 parts of high-white bentonite, and 7 parts of wollastonite. The ceramic tile obtained in the present embodiment contains the following chemical components in weight percentage: Al2O3 20.01%, SiO2 58.31%, Fe2O3 0.06%, TiO2 0.10%, CaO 3.65%, MgO 3.55%, K2O 4.15%, Na2O 3.67%, and the rest are reduced and impurities.

[0079] The glaze in the ceramic tile obtained in this embodiment contains the following chemical components in weight percentage: Al2O3 23.54%, SiO2 50.01%, K2O 3.05%, Na2O 2.62%, CaO 5.20%, MgO 2.25%, BaO 2.44%, ZnO 3.81%, and ZrO 2 7.04%.

[0080] Comparative Example 1

[0081] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that calcined talc is not used in step (2). The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 20.64%, SiO2 60.81%, Fe2O3 0.10%, TiO2 0.15%, CaO 3.94%, MgO 1.08%, K2O 3.88%, Na2O 2.99%, and the rest are reduced and impurities.

[0082] Comparative Example 2

[0083] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that the amount of calcined talc used in step (2) is 8 parts by weight. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 18.54%, SiO2 61.85%, Fe2O3 0.04%, TiO2 0.06%, CaO 2.78%, MgO 5.01%, K2O 3.94%, Na2O 3.50%, and the rest are reduced and impurities.

[0084] Comparative Example 3

[0085] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that the diopside used in step (2) is 1.5 parts by weight. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 19.94%, SiO2 60.51%, Fe2O3 0.04%, TiO2 0.10%, CaO 2.09%, MgO 2.09%, K2O 3.98%, Na2O 3.52%, and the rest are reduced and impurities.

[0086] Comparative Example 4

[0087] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that the diopside used in step (2) is 6 parts by weight. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 18.85%, SiO2 59.79%, Fe2O3 0.05%, TiO2 0.10%, CaO 4.10%, MgO 4.35%, K2O 2.94%, Na2O 2.44%, and the rest are reduced and impurities.

[0088] Comparative Example 5

[0089] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that the calcined coal gangue used in step (2) is 10 parts by weight. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 17.99%, SiO2 58.00%, Fe2O3 0.50%, TiO2 0.12%, CaO 3.37%, MgO 3.60%, K2O 3.97%, Na2O 3.56%, and the rest are reduced and impurities.

[0090] Comparative Example 6

[0091] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that the calcined coal gangue used in step (2) is 33 parts by weight. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 20.62%, SiO2 61.55%, Fe2O3 0.06%, TiO2 0.07%, CaO 2.46%, MgO 3.12%, K2O 3.17%, Na2O 2.17%, and the rest are reduced and impurities.

[0092] Comparative Example 7

[0093] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that in step (2), an equal weight of conventional potassium sodium stone powder is used to completely replace the washed potassium sodium stone powder. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 19.47%, SiO2 59.69%, Fe2O3 0.3%, TiO2 0.07%, CaO 2.07%, MgO 3.09%, K2O 3.55%, Na2O 2.66%, and the rest are reduced and impurities.

[0094] Comparative Example 8

[0095] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that in step (2), an equal weight of conventional sodium stone powder is used to completely replace the water-ground sodium stone powder. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 19.58%, SiO2 59.56%, Fe2O3 0.34%, TiO2 0.07%, CaO 2.94%, MgO 3.24%, K2O 3.77%, Na2O 2.56%, and the rest are reduced and impurities.

[0096] Comparative Example 9

[0097] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that the water-washed potassium-sodium stone powder used in step (2) is 18 parts by weight. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 19.36%, SiO2 59.67%, Fe2O3 0.11%, TiO2 0.13%, CaO 2.67%, MgO 3.36%, K2O 2.79%, Na2O 1.87%, and the rest are reduced and impurities.

[0098] Comparative Example 10

[0099] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that the water-washed potassium-sodium stone powder used in step (2) is 33 parts by weight. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 18.68%, SiO2 58.39%, Fe2O3 0.04%, TiO2 0.11%, CaO 3.21%, MgO 3.09%, K2O 4.74%, Na2O 3.93%, and the rest are reduced and impurities.

[0100] Comparative Example 11

[0101] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that the water-ground sodium stone powder used in step (2) is 49 parts by weight, and no water-washed potassium sodium stone powder is used. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 19.37%, SiO2 59.67%, Fe2O3 0.13%, TiO2 0.09%, CaO 3.26%, MgO 3.04%, K2O 0.79%, Na2O 5.92%, and the rest are reduced and impurities.

[0102] Comparative Example 12

[0103] This comparative example provides a ceramic tile, and its preparation method is different from that of Example 1 in that the water-washed potassium sodium stone powder used in step (2) is 49 parts by weight, and water-ground sodium stone powder is not used. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 17.44%, SiO2 62.31%, Fe2O3 0.06%, TiO2 0.11%, CaO 2.77%, MgO 3.89%, K2O 5.64%, Na2O 1.08%, and the rest are reduced and impurities.

[0104] Comparative Example 13

[0105] This comparative example provides a ceramic tile, the preparation method of which is different from that of Example 1 in that the conventional bentonite of equal weight used in step (2) completely replaces the high white bentonite. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 18.78%, SiO2 59.58%, Fe2O3 0.24%, TiO2 0.31%, CaO 3.55%, MgO 3.28%, K2O 4.11%, Na2O 2.75%, and the rest are reduced and impurities.

[0106] Comparative Example 14

[0107] This comparative example provides a ceramic tile, the preparation method of which is different from that of Example 1 in that the conventional ball clay of equal weight used in step (2) completely replaces the washed ball clay. The green body of the ceramic tile obtained in this comparative example contains the following chemical components in percentage by weight: Al2O3 17.65%, SiO2 61.67%, Fe2O3 0.32%, TiO2 0.44%, CaO 2.21%, MgO 4.15%, K2O 3.58%, Na2O 3.58%, and the rest are reduced and impurities.

[0108] Test Example 1:

[0109] The ceramic tiles obtained from the above examples and comparative examples were subjected to the following performance tests:

[0110] Whiteness test method: Use a digital whiteness meter to directly test the whiteness of ceramic tiles. If the whiteness is above 75°, it is qualified, otherwise it is unqualified;

[0111] Light transmittance test method: shine a light on the back of the ceramic tile and observe whether the front side is light-transmissive;

[0112] Green brick (i.e. dry brick) strength test method: (a) Destructive strength: select sample rock plate, make it into a square shape of 600mm*600mm*10mm, place it in the flexural instrument to measure the destructive strength, set the span to 580mm, gradually apply pressure, and the force data required when the sample breaks is the destructive strength; (b) Rupture modulus: The rupture modulus detection method is the same as the above-mentioned destructive strength test method. After obtaining the destructive strength data, calculate it according to the following formula: Rupture modulus = destructive strength * 580 (i.e. span) * 1.5 / 600 (i.e. sample brick side length) * (square of sample thickness), where the destructive strength unit is N and the sample thickness unit is mm. The rupture modulus is qualified if it is above 1.8MPa, otherwise it is unqualified.

[0113] Table 1

[0114]

[0115] It can be seen from the above data that the green ceramic tiles of each embodiment have both high whiteness and high strength, which makes the ceramic tiles have high whiteness, are not easy to break during the rapid firing process, and have a higher yield rate. The whiteness of the ceramic tiles of each embodiment is above 75°, and the green body rupture modulus is above 1.8MPa. In addition, the ceramic tiles of each embodiment have a slightly light-transmitting effect.

[0116] Comparative Example 1 does not use burnt talc, resulting in a low magnesium oxide content in the green body, low whiteness, opacity, and low strength. Comparative Example 2 uses a large amount of burnt talc, resulting in over-melting, reducing the whiteness of the product, thereby affecting the light transmission effect. Comparative Example 3 uses a low amount of diopside, resulting in insufficient melting after firing, and the green body is milky, which affects the light transmittance and whiteness. Comparative Example 4 uses a high amount of diopside, resulting in excessive MgO content in the green body, excessive high-temperature melting, and excessive crystals, resulting in poor light transmittance. Comparative Example 5 uses less calcined coal gangue, resulting in low whiteness of the main skeleton components, which also affects the light transmittance of the product. Comparative Example 6 uses too much coal gangue, resulting in a high aluminum content in the green body, affecting the light transmittance and strength of the green body. Comparative Example 7 uses conventional potassium sodium stone powder instead of water-washed material, and the high iron content affects the whiteness and light transmittance of the green body. Comparative Example 8 uses conventional sodium stone powder instead of water-washed material, and the high iron content affects the whiteness and light transmittance of the green body. Comparative Example 9 has less water-washed potassium-sodium stone powder, resulting in a higher iron content and low whiteness in the green body, which affects the light transmittance of the green body. Comparative Example 10 has a larger amount of potassium-sodium stone powder, resulting in a high degree of melting of the green body, which reduces the whiteness of the green body, but has more glass phases and is translucent. Comparative Example 11 does not use water-washed potassium-sodium stone powder, resulting in a low potassium content in the formula, which does not achieve the effect of the composite flux, resulting in a low degree of melting, causing the green body to be opaque and opaque. Comparative Example 12 does not use water-ground sodium stone powder, which does not achieve the effect of the composite flux, resulting in a low degree of melting, causing the green body to be opaque and opaque. Comparative Example 13 has a too high iron content in conventional bentonite, resulting in a low whiteness of the green body, affecting the appearance and causing poor light transmittance. Comparative Example 14 uses conventional ball clay, resulting in an excessively high iron content in the formula, which reduces the whiteness of the green body, affecting the appearance and light transmittance.

[0117] The results of light transmittance test of the ceramic tiles of Example 1 and Comparative Example 1 and observing whether the ceramic tiles are light transmittance are as follows: Figure 1 , Figure 2 and Figure 3 shown.

[0118] Figure 1 This is a photo of the light transmission effect of the front side of the ceramic tile in Example 1; Figure 2 This is a photo of the light transmission effect of the back of the ceramic tile in Example 1; Figure 3 This is a photo of the light-transmitting effect of the front side of the ceramic tile of Example 1. Obviously, the front and back sides of the ceramic tile of Example 1 have a slight light-transmitting effect, while the ceramic tile of Example 1 has no light-transmitting effect.

[0119] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A ceramic tile, characterized in that: The ceramic tile comprises a ceramic body, and the ceramic body comprises the following chemical components in weight percentage: Al2O3 19.05% to 19.65%, SiO2 59.24% to 60.87%, Fe2O3 0.06% to 0.07%, TiO2 0.06% to 0.08%, CaO 2.69% to 3.55%, MgO 3.68% to 4.05%, K2O 3.55% to 4.05%, Na2O 2.65% to 3.14%, and the rest are ignition loss and impurities; The raw materials for preparing the ceramic green body include the following components in parts by weight: 7-8 parts of washed ball clay, 23-25 ​​parts of washed calcite powder, 3-5 parts of calcined talc, 2-4 parts of diopside, 17.5-22.5 parts of calcined coal gangue, 18-22 parts of water-ground calcite powder, 12-14 parts of ultra-white sand, 2-4 parts of high-white bentonite, and 3-7 parts of wollastonite, wherein the ultra-white sand has a whiteness of more than 85° after firing, and the high-white bentonite has a whiteness of more than 75° after firing.

2. The ceramic tile according to claim 1, characterized in that The ceramic tile further comprises a glaze layer and a pattern layer; the ceramic body, the glaze layer and the pattern layer are stacked in sequence; The glaze layer includes the following components in weight percentage: Al2O3: 21.05% to 23.54%, SiO2: 49.88% to 52.14%, K2O: 2.34% to 3.65%, Na2O: 2.31% to 3.68%, CaO: 3.65% to 5.34%, MgO: 1.24% to 2.35%, BaO: 2.34% to 5.32%, ZnO: 2.31% to 4.21%, and ZrO2: 6.31% to 8.25%.

3. The ceramic tile according to claim 1, characterized in that: The whiteness of the ceramic body is 75° to 80°.

4. The method for preparing a ceramic tile according to any one of claims 1 to 3, characterized in that: The following steps are involved: Washed ball clay, washed potassium sodium stone powder, burned talc, diopside, calcined coal gangue, water-ground sodium stone powder, super white sand, high white bentonite and wollastonite are mixed, and then water, a water reducing agent and a suspending agent are added, and ball milling is performed to obtain a green body slurry; The obtained green body slurry is subjected to iron removal and spray drying to obtain green body powder; The obtained green body powder is pressed into shape and dried to obtain a dry brick; The obtained dried bricks are glazed, patterned and fired to obtain ceramic tiles.

5. The method for preparing a ceramic tile according to claim 4, characterized in that: At least one of the following conditions is met: (1) In the process of preparing the green body slurry, based on the total weight of the washed ball clay, the washed potassium sodium stone powder, the burned talc, the diopside, the calcined coal gangue, the water-ground sodium stone powder, the ultra-white sand, the high white bentonite and the wollastonite, the weight of the water is 38% to 42%, the weight of the water reducer is 0.25% to 0.35%, and the weight of the suspending agent is 0.15% to 0.20%; (2) The water reducing agent includes sodium tripolyphosphate; (3) The suspending agent includes sodium methylcellulose; (4) The moisture content of the green body powder is 6.5wt.% to 7.0wt.%; (5) The strength of the dried brick is 2.35-2.4 MPa; (6) The sintering temperature is 1185° to 1195° C., and the sintering time is 60 to 70 minutes.

6. Use of the ceramic tile according to any one of claims 1 to 3 in architectural decoration.

7. Use of the ceramic tile according to any one of claims 1 to 3 in background wall decoration.