A method for preparing ultra-high permeability zirconia powder

By using modified stabilizers and composite dispersants in the preparation of zirconia powder, the problems of low permeability and poor corrosion resistance of zirconia powder are solved, and high permeability and excellent wear resistance are achieved.

CN118545995BActive Publication Date: 2024-10-11ZIRDENT NEW MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411017208.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-10-11
Estimated Expiration
2044-07-29

AI Technical Summary

Technical Problem

The existing ultra-high permeability zirconia powder has low permeability, poor corrosion resistance and poor mechanical properties.

Method used

In the preparation process of zirconia powder, modified stabilizers and composite dispersants are used to improve the dispersion and stability of the powder, enhance wear resistance, and improve the uniform dispersion and uniformity of the powder through the composite dispersant. Interfacial compatibility, combined with sintering aids, promotes the sintering process of zirconia powder.

Benefits of technology

It significantly improves the permeability, corrosion resistance and mechanical properties of zirconia powder, forms nano-scale particles, and enhances the structural integrity and interface bonding force of the powder.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses a method for preparing ultra-high permeability zirconium oxide powder, and belongs to the technical field of zirconium oxide powder preparation. The method for preparing ultra-high permeability zirconium oxide powder comprises the following steps: step (1): dissolving zirconium oxychloride in distilled water, and then adding yttrium oxide, a modified stabilizer and aluminum nitrate to obtain a reaction solution A; step (2): dissolving sodium hydroxide in distilled water, and adding a composite dispersant to obtain a reaction solution B; step (3): adding the reaction solution A dropwise to the reaction solution B until the reaction is completed; step (4): standing the mixed liquid obtained by the reaction for aging, washing, drying, and ball milling, and then mixing a sintering aid in anhydrous ethanol evenly, adding the mixture to a ball milling jar for mixing, and continuing ball milling, drying, sieving, and calcining to obtain ultra-high permeability zirconium oxide powder. The zirconium oxide powder obtained by the method has ultra-high permeability, excellent wear resistance and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of zirconium oxide powder preparation, and specifically relates to a method for preparing ultra-high permeability zirconium oxide powder. Background Art

[0002] With the continuous development of science and technology, the requirements for material performance are also increasing. Zirconia, as an important ceramic material, is widely used in various fields due to its high hardness, high melting point, good chemical stability and thermal stability. Ultra-high permeability zirconia powder is an ideal choice for the preparation of high-performance ceramics, optical devices and other materials due to its excellent optical properties.

[0003] At present, the preparation methods of ultra-high permeability zirconium oxide powder mainly include physical method and chemical method. The physical method is mainly prepared by mechanical grinding, solid phase reaction and other methods. Although the process is simple, it is difficult to obtain fine particle size and uniform distribution of powder. The zirconium oxide powder prepared by the chemical method has uniform chemical composition, fine particle size and narrow distribution, but the cost of the raw materials used is high and the production cycle is long.

[0004] Patent CN 104211114 B discloses a method for preparing nano-stabilized zirconium oxide powder, which first dissolves soluble zirconium salt and soluble metal salt as stabilizer additives in deionized water, adds polycarboxylic acid complexing agent after they are completely dissolved, and adjusts the pH value, then adds polyol crosslinking agent, heats in a water bath, and converts the solution into colloid through esterification reaction; slurries the colloid and dispersant to obtain slurry that can be transported by a pump; atomizes and dries the slurry; and fully burns the dried material under the action of oxygen to obtain nano-stabilized zirconium oxide powder. The product has the advantages of small particle size, narrow particle size distribution, uniform composition, good dispersibility, and high powder crystallinity, but the permeability, corrosion resistance and mechanical properties of the zirconium oxide powder prepared by this method still have room for improvement. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing ultra-high permeability zirconium oxide powder, which is used to solve the technical problems of low permeability, poor corrosion resistance and poor mechanical properties of zirconium oxide powder in the prior art.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The present invention provides a method for preparing ultra-high permeability zirconium oxide powder, comprising the following steps:

[0008] Step (1): dissolving zirconium oxychloride in distilled water, then adding yttrium oxide, a modified stabilizer and aluminum nitrate, stirring and mixing to obtain a reaction solution A;

[0009] Step (2): dissolving sodium hydroxide in distilled water, adding a composite dispersant, mixing and stirring to obtain a reaction solution B;

[0010] Step (3): placing the reaction solution B in a heat-collecting constant temperature heating magnetic stirrer, and then adding the reaction solution A dropwise into the reaction solution B until the reaction is completed;

[0011] Step (4): The mixed liquid obtained by the reaction is allowed to stand for aging, washed, dried, and ball-milled. The sintering aid is then mixed evenly in anhydrous ethanol and added to a ball mill for mixing. The mixture is then ball-milled, dried, sieved, and calcined to obtain an ultra-high permeability zirconium oxide powder.

[0012] Preferably, in step (1), the dosage ratio of zirconium oxychloride, distilled water, yttrium oxide, modified stabilizer and aluminum nitrate is (60-70) g: (1-1.5) L: (2.416-2.484) g: (1.8-2.1) g: (1.8-2.1) g, and the stirring and mixing time is 30-40 min.

[0013] Preferably, the preparation method of the modified stabilizer comprises the following steps:

[0014] Q1: Add 2-chloro-2-oxo-1,3,2-dioxaphospholane to triethylamine, then add 3-butyn-1-ol and tetrahydrofuran, and react under ice bath conditions to obtain intermediate product 1; add dichloromethane to a container, then add 1,8-diazacyclo[5,4,0]undecene-7, introduce nitrogen, add intermediate product 1 and N-BOC-ethanolamine, mix well, react at low temperature, add glacial acetic acid dropwise to terminate the reaction, continue stirring, rotary evaporate, precipitate, and dry to obtain intermediate product 2;

[0015] Q2: Add the intermediate product 2 to a container filled with dichloromethane, stir to dissolve, add dichloromethane and trifluoroacetic acid to a constant pressure dropping funnel, mix well, add dropwise to the container, stir, rotary evaporate, precipitate, and dry to obtain the intermediate product 3;

[0016] Q3: Ultrasonic dispersion of cellulose nanocrystals in deionized water, then adding 2,2,6,6-tetramethylpiperidinyl oxide and sodium bromide, adjusting the pH, and then dropping sodium hypochlorite solution. After the addition is complete, the pH is adjusted, stirring is continued, methanol is added, stirring is continued, the pH is adjusted, stirring is continued, and then the suspension is centrifuged, the upper liquid is taken out, precipitated, centrifuged, washed, dialyzed, and freeze-dried to obtain intermediate 4;

[0017] Q4: Add the intermediate product 4 to a container filled with N,N-dimethylformamide, and after ultrasonic dispersion, add 1-(3-dimethylaminopropyl)-3-cyclohexylcarbodiimide to activate the carboxyl group, and then add N-hydroxysuccinimide. Continue stirring, dissolve the intermediate product 3 in N,N-dimethylformamide, and slowly add it dropwise to the container. After the reaction is completed, heat to extract N,N-dimethylformamide, precipitate, centrifuge, wash, dialyze, and freeze-dry to obtain a modified stabilizer.

[0018] In the above process, 2-chloro-2-oxo-1,3,2-dioxaphospholane and 3-butyn-1-ol are first subjected to a substitution reaction to generate an intermediate product 1, and then the intermediate product 3 is grafted onto the surface of the cellulose nanocrystal through a ring-opening polymerization and hydrolysis reaction of the intermediate product 1 and an oxidation and amidation reaction of the cellulose nanocrystal to obtain a modified stabilizer, wherein the synthetic reaction formula of the modified stabilizer is as follows:

[0019]

[0020] After mass spectrometry analysis, the results of intermediate 1 were: m / z: 176.02 (100.0%), 177.03 (6.7%), 178.03 (1.0%).

[0021] Preferably, in Q1, the molar ratio of 2-chloro-2-oxo-1,3,2-dioxaphospholane and 3-butyn-1-ol is (0.8-1.1): (0.9-1.2), the reaction time is 12-14h, the molar ratio of 1,8-diazacyclo[5,4,0]undecene-7, intermediate 1 and N-BOC-ethanolamine is (3.41-6.82): (8.25-16.50): (1.71-3.42), and the low temperature reaction temperature is -10~-15 ℃, reaction time is 30-45min, stirring time is 30-35min, drying temperature is 25-30℃, and time is 48-60h; in Q2, the amount ratio of intermediate product 2, dichloromethane, dichloromethane and trifluoroacetic acid in the constant pressure dropping funnel is (1.04-2.08)g: (10-20)mL: (10-20)mL: (3-6)mL, the dropping temperature is -5~-8℃, the dropping time is 30-45min, the stirring time is 12-14h, the drying temperature is 25-30℃, and the time is 48-50h.

[0022] Preferably, in Q3, the amount ratio of cellulose nanocrystals, deionized water, 2,2,6,6-tetramethylpiperidinium oxide, sodium bromide, sodium hypochlorite and methanol is (3-6) g: (300-600) mL: (60-120) mg: (1.20-2.40) g: (33.10-66.22) g: (30-60) mL, the pH is adjusted to 5.6 with 0.5 mol / L sodium hydroxide for the first time, and the time for adding sodium hypochlorite solution is 30-40 min, the pH is adjusted to 10 with 0.5 mol / L sodium hydroxide for the second time, the stirring time is 12-14 h, the stirring time is continued for 1-2 h, and the third time is 1 mol / L sodium hydroxide. / L of hydrochloric acid to adjust the pH to 1, continue stirring for 24-30 hours, and the dialysis time is 72-84 hours; in Q4, the mass ratio of intermediate 4, 1-(3-dimethylaminopropyl)-3-cyclohexylcarbodiimide, N-hydroxysuccinimide, and intermediate 3 is (100.1-200.3) mg: (433.3-866.4) mg: (260.7-521.2) mg: (1.42-2.88) g, the carboxyl activation time is 30-40 minutes, the stirring time is continued for 12-14 hours, the reaction temperature is 28-30°C, the time is 24-36 hours, the heating temperature is 65-70°C, and the dialysis time is 72-84 hours.

[0023] Preferably, in step (2), the dosage ratio of sodium hydroxide, distilled water and composite dispersant is (1.6-2.4) g: (1-1.5) L: (0.032-0.048) g, and the mixing and stirring time is 20-30 min.

[0024] Preferably, the preparation method of the composite dispersant comprises the following steps:

[0025] S1: adding glycidyl methacrylate to deionized water, heating to reflux, and freeze-drying to obtain 2,3-dihydroxy methacrylate;

[0026] S2: Add acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid, 2,3-dihydroxymethylacrylate, thioglycolic acid and deionized water into a container, heat, and under nitrogen protection, dropwise add an aqueous solution of ammonium persulfate, control the dropping time, and after the dropping is completed, increase the temperature to react. After the reaction is completed, cool down and adjust the pH to obtain a composite dispersant.

[0027] In the above process, the synthetic reaction formula of the composite dispersant is as follows:

[0028]

[0029] Preferably, in S1, the dosage ratio of glycidyl methacrylate to deionized water is (4.95-7.43) g: (50-75) mL, the heating reflux temperature is 80-90° C., and the time is 9-10 h; in S2, the dosage ratio of acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid, 2,3-dihydroxymethylacrylate, thioglycolic acid, deionized water and ammonium persulfate aqueous solution is (7.26-9.44 )g: (20.7-26.91)g: (1.6-2.08)g: (1.84-2.39)g: (41-53.3)mL: (5-7.5)mL, the heating temperature is 60-70℃, the concentration of the ammonium persulfate aqueous solution is 0.177g / mL, the dropping time is 20-30min, the heating temperature is 70-80℃, and the pH is adjusted to 7.0-8.0 with 40wt% sodium hydroxide solution.

[0030] Preferably, in step (3), the temperature of the heat-collecting constant temperature heating magnetic stirrer is 60-70°C, and the stirring rate is 800-1000 rpm, until the pH value is 8-10, and the reaction is completed.

[0031] Preferably, in step (4), the aging time is 90-150 min, the drying temperature is 80-90°C, the time is 12-14 h, the sintering aid is a mixture of calcium oxide and yttrium trioxide, the ball milling speed is 300-400 rpm, the ball milling time is 180-240 min, the calcination temperature is 500-700°C, and the calcination time is 4-6 h.

[0032] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:

[0033] 1. The present invention first adds the prepared modified stabilizer and composite dispersant into the preparation process of zirconium oxide powder, which can improve the dispersibility and stability of zirconium oxide powder in the solvent, prevent particle agglomeration, and improve the uniformity of the powder, so that the prepared zirconium oxide powder has ultra-high permeability. At the same time, the presence of the modified stabilizer can also increase the wear resistance of the zirconium oxide powder. Subsequently, the sintering aid and anhydrous ethanol are evenly mixed and mixed with the zirconium oxide powder to promote the sintering process, so that a strong bonding force is formed between the zirconium oxide powder particles, and its corrosion resistance and mechanical properties are improved.

[0034] 2. The present invention uses 2-chloro-2-oxo-1,3,2-dioxaphospholane, 3-butyne-1-ol, 1,8-diazacyclo[5,4,0]undecene-7, N-BOC-ethanolamine and cellulose nanocrystals as raw materials to prepare a modified stabilizer. Adding it to the preparation process of zirconium oxide powder can effectively improve the dispersibility and stability of the powder in the solvent, so that the obtained zirconium oxide powder presents a nano form, and its grain size is reduced to the nanoscale, which helps to reduce light scattering and increase light transmittance, improve the permeability of the zirconium oxide powder, and at the same time, improve the interface bonding between the zirconium oxide powder and the organic matrix, and enhance the interface compatibility. The presence of the modified stabilizer can also enhance the wear resistance by enhancing the structural integrity of the zirconium oxide powder or improving the bonding force between the grains.

[0035] 3. The present invention uses glycidyl methacrylate, acrylic acid and 2-acrylamide-2-methylpropane sulfonic acid as raw materials to synthesize a composite dispersant. When the composite dispersant is added to the preparation process of zirconium oxide powder, the functional groups in the composite dispersant can quickly react with the polar groups on the surface of the zirconium oxide powder to form stable chemical bonds, which is conducive to the uniform dispersion of the powder and can also increase the fluidity and stability of the slurry. The hydrophilic groups in the composite dispersant can also enhance its wettability to the zirconium oxide powder, making the powder easier to be wrapped and dispersed by the medium, thereby reducing the viscosity of the slurry and improving production efficiency. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] The following embodiments of the present invention are used:

[0038] 2-Chloro-2-oxo-1,3,2-dioxaphospholane was purchased from Yangzhou Modier Electronic Materials Co., Ltd., CAS No.: 6609-64-9;

[0039] Triethylamine was purchased from Shandong Mingyu Supply Chain Management Co., Ltd., CAS No.: 121-44-8;

[0040] 3-Butyn-1-ol was purchased from Nantong Runfeng Petrochemical Co., Ltd., CAS No.: 927-74-2;

[0041] Tetrahydrofuran was purchased from Shandong Mantanghong New Materials Co., Ltd., CAS No.: 109-99-9;

[0042] Dichloromethane was purchased from Jinan Weizhen Chemical Co., Ltd., CAS No.: 75-09-2;

[0043] 1,8-Diazacyclo[5,4,0]undecene-7 was purchased from Shanghai Bangcheng Chemical Co., Ltd., CAS No.: 6674-22-2;

[0044] N-BOC-ethanolamine was purchased from Wuhan Xinyang Ruihe Chemical Technology Co., Ltd., CAS No.: 26690-80-2;

[0045] Glacial acetic acid was purchased from Shandong Huayu Chemical Technology Co., Ltd., CAS No.: 64-19-7;

[0046] Trifluoroacetic acid was purchased from Shandong Shengcang Chemical Technology Co., Ltd., CAS No.: 76-05-1;

[0047] Cellulose nanocrystals were purchased from Beijing Shansi Technology Co., Ltd.;

[0048] 2,2,6,6-Tetramethylpiperidinyl oxide was purchased from Nantong Runfeng Petrochemical Co., Ltd., CAS No.: 2564-83-2;

[0049] Sodium bromide was purchased from Weifang Youlan Chemical Co., Ltd., CAS No.: 7647-15-6;

[0050] Sodium hypochlorite was purchased from Jinan Xichuan Chemical Technology Co., Ltd., CAS No.: 7681-52-9;

[0051] Methanol was purchased from Tianjin Jindong Tianzheng Fine Chemical Reagent Factory, CAS No.: 67-56-1;

[0052] Hydrochloric acid was purchased from Jiangsu Xuhong Environmental Protection Technology Co., Ltd., CAS No.: 7647-01-0;

[0053] N,N-dimethylformamide was purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., CAS No.: 68-12-2;

[0054] 1-(3-Dimethylaminopropyl)-3-cyclohexylcarbodiimide was purchased from Sane Chemical Technology (Shanghai) Co., Ltd., CAS No.: 59457-43-1;

[0055] N-Hydroxysuccinimide was purchased from Jiangsu Bosite Chemical Technology Co., Ltd., CAS No.: 6066-82-6;

[0056] Glycidyl methacrylate was purchased from Jinan Shuangying Chemical Co., Ltd., CAS No.: 106-91-2;

[0057] Acrylic acid was purchased from Shandong Mingyue Chemical Co., Ltd., CAS No.: 79-10-7;

[0058] 2-Acrylamide-2-methylpropanesulfonic acid was purchased from Shandong Xinghai Chemical Co., Ltd., CAS No.: 15214-89-8;

[0059] Thioglycolic acid was purchased from Shandong Jinghao Chemical Co., Ltd., CAS No.: 68-11-1;

[0060] Ammonium persulfate was purchased from Shandong Jinli Chemical Co., Ltd., CAS number: 7727-54-0;

[0061] Zirconium oxychloride was purchased from Zibo Huantuo Biotechnology Co., Ltd., CAS number: 7699-43-6;

[0062] Yttrium oxide was purchased from Langfang Qianyao Technology Co., Ltd., CAS No.: 1314-36-9;

[0063] Aluminum nitrate was purchased from Shandong Xinhongrui Chemical Co., Ltd., CAS No.: 13473-90-0;

[0064] Calcium oxide was purchased from Langfang Pengcai Fine Chemical Co., Ltd., CAS No.: 1305-78-8;

[0065] Yttrium trioxide was purchased from Jinan Rongzheng Chemical Co., Ltd., CAS No.: 1314-36-9;

[0066] Anhydrous ethanol was purchased from Guangzhou Xinyang Chemical Co., Ltd., CAS No.: 64-17-5.

[0067] Example 1

[0068] This embodiment discloses a method for preparing a modified stabilizer, comprising the following steps:

[0069] Q1: Add 2.55 mL of 2-chloro-2-oxo-1,3,2-dioxaphospholane to triethylamine, then add 2.08 mL of 3-butyn-1-ol and tetrahydrofuran, and react for 12 h in an ice bath to obtain intermediate 1; add dichloromethane to a container, then add 0.778 g of 1,8-diazacyclo[5,4,0]undecene-7, pass nitrogen, add 2.264 g of intermediate 1 and 0.413 g of N-BOC-ethanolamine, mix well, react at -15 °C for 45 min, add glacial acetic acid to terminate the reaction, continue stirring for 30 min, rotary evaporate, precipitate, and dry at 30 °C for 48 h to obtain intermediate 2;

[0070] Q2: Add 1.56 g of intermediate product 2 to a container containing 15 mL of dichloromethane, stir to dissolve, add 15 mL of dichloromethane and 4.5 mL of trifluoroacetic acid to a constant pressure dropping funnel, mix well, and then add dropwise to the container at -8°C for 30 min. Stir for 14 h, rotary evaporate, precipitate, and dry at 30°C for 48 h to obtain intermediate product 3;

[0071] Q3: 4.5 g of cellulose nanocrystals were ultrasonically dispersed in 450 mL of deionized water, and then 90 mg of 2,2,6,6-tetramethylpiperidinoxide and 1.80 g of sodium bromide were added. After adjusting the pH to 5.6 with 0.5 mol / L of sodium hydroxide, 49.66 g of sodium hypochlorite solution was added dropwise for 30 min. After the addition was completed, the pH was adjusted to 10 with 0.5 mol / L of sodium hydroxide, and the mixture was stirred for 12 h. 45 mL of methanol was added, and the mixture was stirred for 2 h. The pH was adjusted to 1 with 1 mol / L of hydrochloric acid, and the mixture was stirred for 30 h. The suspension was then centrifuged, the upper liquid was taken out, precipitated, centrifuged, washed, dialyzed for 72 h, and freeze-dried to obtain intermediate 4.

[0072] Q4: Add 150.2 mg of intermediate product 4 to a container filled with N,N-dimethylformamide. After ultrasonic dispersion, add 649.9 mg of 1-(3-dimethylaminopropyl)-3-cyclohexylcarbodiimide to activate the carboxyl group for 30 minutes, then add 391.0 mg of N-hydroxysuccinimide and continue stirring for 12 hours. Dissolve 2.15 g of intermediate product 3 in N,N-dimethylformamide and slowly add it dropwise to the container. React at 30°C for 36 hours. After the reaction is completed, heat to 70°C to extract N,N-dimethylformamide, precipitate, centrifuge, wash, dialyze for 72 hours, and freeze-dry to obtain a modified stabilizer.

[0073] This embodiment discloses a method for preparing a composite dispersant, comprising the following steps:

[0074] S1: 6.19 g of glycidyl methacrylate was added to 62.5 mL of deionized water, heated under reflux at 90 °C for 10 h, and freeze-dried to obtain 2,3-dihydroxy methacrylate;

[0075] S2: 8.35g acrylic acid, 23.3g 2-acrylamide-2-methylpropanesulfonic acid, 1.84g 2,3-dihydroxymethylacrylate, 2.12g thioglycolic acid and 47.15mL deionized water were added to a container, heated at 70°C, and under nitrogen protection, 6.25mL 0.177g / mL ammonium persulfate aqueous solution was added dropwise, and the dropping time was controlled to be 30min. After the dropping was completed, the temperature was raised to 80°C for reaction. After the reaction was completed, the temperature was lowered and the pH was adjusted to 7.0 with 40wt% sodium hydroxide solution to obtain a composite dispersant.

[0076] This embodiment discloses a method for preparing ultra-high permeability zirconium oxide powder, comprising the following steps:

[0077] Step (1): dissolving 65 g of zirconium oxychloride in 1.25 L of distilled water, then adding 2.450 g of yttrium oxide, 1.9 g of a modified stabilizer and 1.8 g of aluminum nitrate, stirring and mixing for 30 minutes to obtain a reaction solution A;

[0078] Step (2): dissolve 2.0 g of sodium hydroxide in 1.25 L of distilled water, add 0.040 g of a composite dispersant, and mix and stir for 30 min to obtain a reaction solution B;

[0079] Step (3): Place the reaction solution B in a heat-collecting constant temperature heating magnetic stirrer at 70°C with a stirring rate of 800 rpm, and then dropwise add the reaction solution A into the reaction solution B until the pH reaches 9 and the reaction is complete;

[0080] Step (4): The mixed liquid obtained by the reaction is allowed to stand for 150 minutes, washed, dried at 90°C for 14 hours, and ball-milled. Then, the mixture of calcium oxide and yttrium trioxide is mixed evenly in anhydrous ethanol, added to a ball mill for mixing, and ball milling is continued for 200 minutes at a ball mill speed of 300 rpm. The mixture is dried, sieved, and calcined at 700°C for 6 hours to obtain ultra-high permeability zirconium oxide powder.

[0081] Example 2

[0082] This embodiment discloses a method for preparing a modified stabilizer, comprising the following steps:

[0083] Q1: Add 2.14 mL of 2-chloro-2-oxo-1,3,2-dioxaphospholane to triethylamine, then add 2 mL of 3-butyn-1-ol and tetrahydrofuran, and react for 12 h in an ice bath to obtain intermediate 1; add dichloromethane to a container, then add 0.519 g of 1,8-diazacyclo[5,4,0]undecene-7, pass nitrogen, add 1.509 g of intermediate 1 and 0.275 g of N-BOC-ethanolamine, mix well, react at -15°C for 45 min, add glacial acetic acid to terminate the reaction, continue stirring for 30 min, rotary evaporate, precipitate, and dry at 30°C for 48 h to obtain intermediate 2;

[0084] Q2: Add 1.04 g of intermediate product 2 to a container containing 10 mL of dichloromethane, stir to dissolve, add 10 mL of dichloromethane and 3 mL of trifluoroacetic acid to a constant pressure dropping funnel, mix well, and then add dropwise to the container at -8°C for 30 min. Stir for 14 h, rotary evaporate, precipitate, and dry at 30°C for 48 h to obtain intermediate product 3.

[0085] Q3: 3 g of cellulose nanocrystals were ultrasonically dispersed in 300 mL of deionized water, and then 60 mg of 2,2,6,6-tetramethylpiperidinyl oxide and 1.20 g of sodium bromide were added. After adjusting the pH to 5.6 with 0.5 mol / L sodium hydroxide, 33.10 g of sodium hypochlorite solution was added dropwise for 30 min. After the addition was completed, the pH was adjusted to 10 with 0.5 mol / L sodium hydroxide, and the mixture was stirred for 12 h. 30 mL of methanol was added, and the stirring was continued for 2 h. The pH was adjusted to 1 with 1 mol / L hydrochloric acid, and the stirring was continued for 30 h. The suspension was then centrifuged, the upper liquid was taken out, precipitated, centrifuged, washed, dialyzed for 72 h, and freeze-dried to obtain intermediate 4.

[0086] Q4: Add 100.1 mg of intermediate product 4 to a container filled with N,N-dimethylformamide. After ultrasonic dispersion, add 433.3 mg of 1-(3-dimethylaminopropyl)-3-cyclohexylcarbodiimide to activate the carboxyl group for 30 minutes, then add 260.7 mg of N-hydroxysuccinimide and continue stirring for 12 hours. Dissolve 1.42 g of intermediate product 3 in N,N-dimethylformamide and slowly add it dropwise to the container. React at 30°C for 36 hours. After the reaction is completed, heat to 70°C to extract N,N-dimethylformamide, precipitate, centrifuge, wash, dialyze for 72 hours, and freeze-dry to obtain a modified stabilizer.

[0087] This embodiment discloses a method for preparing a composite dispersant, comprising the following steps:

[0088] S1: 4.95 g of glycidyl methacrylate was added to 50 mL of deionized water, heated under reflux at 90 °C for 10 h, and freeze-dried to obtain 2,3-dihydroxy methacrylate;

[0089] S2: 7.26 g of acrylic acid, 20.7 g of 2-acrylamide-2-methylpropanesulfonic acid, 1.6 g of 2,3-dihydroxymethylacrylate, 1.84 g of thioglycolic acid and 41 mL of deionized water were added to a container, heated at 70°C, and under nitrogen protection, 5 mL of 0.177 g / mL ammonium persulfate aqueous solution was added dropwise, and the dropping time was controlled to be 30 min. After the dropping was completed, the temperature was raised to 80°C for reaction. After the reaction was completed, the temperature was lowered and the pH was adjusted to 7.0 with 40 wt% sodium hydroxide solution to obtain a composite dispersant.

[0090] This embodiment discloses a method for preparing ultra-high permeability zirconium oxide powder, comprising the following steps:

[0091] Step (1): dissolving 60 g of zirconium oxychloride in 1 L of distilled water, then adding 2.416 g of yttrium oxide, 1.8 g of a modified stabilizer and 2.1 g of aluminum nitrate, stirring and mixing for 30 minutes to obtain a reaction solution A;

[0092] Step (2): dissolve 1.6 g of sodium hydroxide in 1 L of distilled water, add 0.032 g of a composite dispersant, and mix and stir for 30 min to obtain a reaction solution B;

[0093] Step (3): Place the reaction solution B in a heat-collecting constant temperature heating magnetic stirrer at 70°C with a stirring rate of 800 rpm, and then dropwise add the reaction solution A into the reaction solution B until the pH reaches 9 and the reaction is complete;

[0094] Step (4): The mixed liquid obtained by the reaction is allowed to stand for 150 minutes, washed, dried at 90°C for 14 hours, and ball-milled. Then, the mixture of calcium oxide and yttrium trioxide is mixed evenly in anhydrous ethanol, added to a ball mill for mixing, and ball milling is continued for 200 minutes at a ball mill speed of 300 rpm. The mixture is dried, sieved, and calcined at 700°C for 6 hours to obtain ultra-high permeability zirconium oxide powder.

[0095] Example 3

[0096] This embodiment discloses a method for preparing a modified stabilizer, comprising the following steps:

[0097] Q1: Add 2.96 mL of 2-chloro-2-oxo-1,3,2-dioxaphospholane to triethylamine, then add 2.16 mL of 3-butyn-1-ol and tetrahydrofuran, and react for 12 h in an ice bath to obtain intermediate 1; add dichloromethane to a container, then add 1.038 g of 1,8-diazacyclo[5,4,0]undecene-7, pass nitrogen, add 3.018 g of intermediate 1 and 0.55 g of N-BOC-ethanolamine, mix well, react at -15 °C for 45 min, add glacial acetic acid to terminate the reaction, continue stirring for 30 min, rotary evaporate, precipitate, and dry at 30 °C for 48 h to obtain intermediate 2;

[0098] Q2: Add 2.08 g of intermediate product 2 to a container containing 12 mL of dichloromethane, stir to dissolve, add 18 mL of dichloromethane and 6 mL of trifluoroacetic acid to a constant pressure dropping funnel, mix well, and then add dropwise to the container at -8 °C for 30 min. Stir for 14 h, rotary evaporate, precipitate, and dry at 30 °C for 48 h to obtain intermediate product 3.

[0099] Q3: 6 g of cellulose nanocrystals were ultrasonically dispersed in 600 mL of deionized water, and then 120 mg of 2,2,6,6-tetramethylpiperidinyl oxide and 1.40 g of sodium bromide were added. After adjusting the pH to 5.6 with 0.5 mol / L sodium hydroxide, 66.22 g of sodium hypochlorite solution was added dropwise for 30 min. After the addition was completed, the pH was adjusted to 10 with 0.5 mol / L sodium hydroxide, and the mixture was stirred for 12 h. 60 mL of methanol was added, and the stirring was continued for 2 h. The pH was adjusted to 1 with 1 mol / L hydrochloric acid, and the stirring was continued for 30 h. The suspension was then centrifuged, the upper liquid was taken out, precipitated, centrifuged, washed, dialyzed for 72 h, and freeze-dried to obtain intermediate 4.

[0100] Q4: Add 200.3 mg of intermediate product 4 to a container filled with N,N-dimethylformamide. After ultrasonic dispersion, add 866.4 mg of 1-(3-dimethylaminopropyl)-3-cyclohexylcarbodiimide to activate the carboxyl group for 30 minutes, then add 521.2 mg of N-hydroxysuccinimide and continue stirring for 12 hours. Dissolve 2.88 g of intermediate product 3 in N,N-dimethylformamide and slowly add it dropwise to the container. React at 30°C for 36 hours. After the reaction is completed, heat to 70°C to extract N,N-dimethylformamide, precipitate, centrifuge, wash, dialyze for 72 hours, and freeze-dry to obtain a modified stabilizer.

[0101] This embodiment discloses a method for preparing a composite dispersant, comprising the following steps:

[0102] S1: 7.43 g of glycidyl methacrylate was added to 75 mL of deionized water, heated under reflux at 90 °C for 10 h, and freeze-dried to obtain 2,3-dihydroxy methacrylate;

[0103] S2: 9.44 g acrylic acid, 26.91 g 2-acrylamide-2-methylpropanesulfonic acid, 2.08 g 2,3-dihydroxymethylacrylate, 2.39 g thioglycolic acid and 53.3 mL deionized water were added to a container, heated at 70°C, and under nitrogen protection, 7.5 mL 0.177 g / mL ammonium persulfate aqueous solution was added dropwise, and the dropping time was controlled to be 30 min. After the dropping was completed, the temperature was raised to 80°C for reaction. After the reaction was completed, the temperature was lowered and the pH was adjusted to 7.0 with 40 wt% sodium hydroxide solution to obtain a composite dispersant.

[0104] This embodiment discloses a method for preparing ultra-high permeability zirconium oxide powder, comprising the following steps:

[0105] Step (1): dissolving 70 g of zirconium oxychloride in 1.5 L of distilled water, then adding 2.484 g of yttrium oxide, 2.1 g of a modified stabilizer and 1.9 g of aluminum nitrate, stirring and mixing for 30 minutes to obtain a reaction solution A;

[0106] Step (2): dissolve 2.4 g of sodium hydroxide in 1.5 L of distilled water, add 0.048 g of a composite dispersant, mix and stir for 30 min, and obtain a reaction solution B;

[0107] Step (3): Place the reaction solution B in a heat-collecting constant temperature heating magnetic stirrer at 70°C with a stirring rate of 800 rpm, and then dropwise add the reaction solution A into the reaction solution B until the pH reaches 9 and the reaction is complete;

[0108] Step (4): The mixed liquid obtained by the reaction is allowed to stand for 150 minutes, washed, dried at 90°C for 14 hours, and ball-milled. Then, the mixture of calcium oxide and yttrium trioxide is mixed evenly in anhydrous ethanol, added to a ball mill for mixing, and ball milling is continued for 200 minutes at a ball mill speed of 300 rpm. The mixture is dried, sieved, and calcined at 700°C for 6 hours to obtain ultra-high permeability zirconium oxide powder.

[0109] Example 4

[0110] This embodiment discloses a method for preparing a modified stabilizer, comprising the following steps:

[0111] Q1: Add 2.28 mL of 2-chloro-2-oxo-1,3,2-dioxaphospholane to triethylamine, then add 2.02 mL of 3-butyn-1-ol and tetrahydrofuran, and react for 12 h in an ice bath to obtain intermediate 1; add dichloromethane to a container, then add 0.624 g of 1,8-diazacyclo[5,4,0]undecene-7, pass nitrogen, add 1.853 g of intermediate 1 and 0.347 g of N-BOC-ethanolamine, mix well, react at -15 °C for 45 min, add glacial acetic acid to terminate the reaction, continue stirring for 30 min, rotary evaporate, precipitate, and dry at 30 °C for 48 h to obtain intermediate 2;

[0112] Q2: Add 1.3 g of intermediate product 2 to a container containing 18 mL of dichloromethane, stir to dissolve, add 12 mL of dichloromethane and 5 mL of trifluoroacetic acid to a constant pressure dropping funnel, mix well, and then add dropwise to the container at -8 °C for 30 min. Stir for 14 h, rotary evaporate, precipitate, and dry at 30 °C for 48 h to obtain intermediate product 3.

[0113] Q3: 4 g of cellulose nanocrystals were ultrasonically dispersed in 500 mL of deionized water, and then 80 mg of 2,2,6,6-tetramethylpiperidinoxide and 1.30 g of sodium bromide were added. After adjusting the pH to 5.6 with 0.5 mol / L sodium hydroxide, 41.33 g of sodium hypochlorite solution was added dropwise for 30 min. After the addition was completed, the pH was adjusted to 10 with 0.5 mol / L sodium hydroxide, and the mixture was stirred for 12 h. 40 mL of methanol was added, and the mixture was stirred for 2 h. The pH was adjusted to 1 with 1 mol / L hydrochloric acid, and the mixture was stirred for 30 h. The suspension was then centrifuged, the upper liquid was taken out, precipitated, centrifuged, washed, dialyzed for 72 h, and freeze-dried to obtain intermediate 4.

[0114] Q4: Add 120.1 mg of intermediate product 4 to a container filled with N,N-dimethylformamide. After ultrasonic dispersion, add 578.1 mg of 1-(3-dimethylaminopropyl)-3-cyclohexylcarbodiimide to activate the carboxyl group for 30 minutes, then add 318.5 mg of N-hydroxysuccinimide and continue stirring for 12 hours. Dissolve 1.87 g of intermediate product 3 in N,N-dimethylformamide and slowly add it dropwise to the container. React at 30°C for 36 hours. After the reaction is completed, heat to 70°C to extract N,N-dimethylformamide, precipitate, centrifuge, wash, dialyze for 72 hours, and freeze-dry to obtain a modified stabilizer.

[0115] This embodiment discloses a method for preparing a composite dispersant, comprising the following steps:

[0116] S1: 5.57 g of glycidyl methacrylate was added to 54 mL of deionized water, heated under reflux at 90 °C for 10 h, and freeze-dried to obtain 2,3-dihydroxy methacrylate;

[0117] S2: 7.81g acrylic acid, 21.75g ​​2-acrylamide-2-methylpropanesulfonic acid, 1.71g 2,3-dihydroxymethylacrylate, 2.27g thioglycolic acid and 44.25mL deionized water were added to a container, heated at 70°C, and under nitrogen protection, 6mL of 0.177g / mL ammonium persulfate aqueous solution was added dropwise, and the dropping time was controlled to be 30min. After the dropping was completed, the temperature was raised to 80°C for reaction. After the reaction was completed, the temperature was lowered and the pH was adjusted to 7.0 with 40wt% sodium hydroxide solution to obtain a composite dispersant.

[0118] This embodiment discloses a method for preparing ultra-high permeability zirconium oxide powder, comprising the following steps:

[0119] Step (1): dissolving 62 g of zirconium oxychloride in 1.1 L of distilled water, then adding 2.423 g of yttrium oxide, 1.85 g of a modified stabilizer and 2.05 g of aluminum nitrate, stirring and mixing for 30 minutes to obtain a reaction solution A;

[0120] Step (2): dissolving 2.2 g of sodium hydroxide in 1.2 L of distilled water, adding 0.036 g of a composite dispersant, and mixing and stirring for 30 min to obtain a reaction solution B;

[0121] Step (3): Place the reaction solution B in a heat-collecting constant temperature heating magnetic stirrer at 70°C with a stirring rate of 800 rpm, and then dropwise add the reaction solution A into the reaction solution B until the pH reaches 9 and the reaction is complete;

[0122] Step (4): The mixed liquid obtained by the reaction is allowed to stand for 150 minutes, washed, dried at 90°C for 14 hours, and ball-milled. Then, the mixture of calcium oxide and yttrium trioxide is mixed evenly in anhydrous ethanol, added to a ball mill for mixing, and ball milling is continued for 200 minutes at a ball mill speed of 300 rpm. The mixture is dried, sieved, and calcined at 700°C for 6 hours to obtain ultra-high permeability zirconium oxide powder.

[0123] Comparative Example 1

[0124] Comparative Example 1 Compared with Example 1, in the process of preparing the modified stabilizer in Comparative Example 1, 2-chloro-2-oxo-1,3,2-dioxaphospholane was not added, and other conditions remained unchanged.

[0125] Comparative Example 2

[0126] Comparative Example 2 Compared with Example 1, in the process of preparing the modified stabilizer in Comparative Example 2, 1,8-diazacyclo[5,4,0]undecene-7 was not added, and other conditions remained unchanged.

[0127] Comparative Example 3

[0128] Comparative Example 3 Compared with Example 1, in the process of preparing the modified stabilizer in Comparative Example 3, no cellulose nanocrystals are added, and other conditions remain unchanged.

[0129] Comparative Example 4

[0130] Comparative Example 4 Compared with Example 1, in the process of preparing the composite dispersant in Comparative Example 4, glycidyl methacrylate was not added, and other conditions remained unchanged.

[0131] Comparative Example 5

[0132] Comparative Example 5 Compared with Example 1, in the process of preparing the composite dispersant in Comparative Example 5, 2-acrylamide-2-methylpropanesulfonic acid was not added, and other conditions remained unchanged.

[0133] Comparative Example 6

[0134] Comparative Example 6 Compared with Example 1, in the process of preparing the composite dispersant in Comparative Example 6, no thioglycolic acid was added, and other conditions remained unchanged.

[0135] Comparative Example 7

[0136] Compared with Example 1, in Comparative Example 7, during the preparation of zirconium oxide powder, no modified stabilizer was added, and other conditions remained unchanged.

[0137] Comparative Example 8

[0138] Compared with Example 1, in Comparative Example 8, during the preparation of zirconium oxide powder, no composite dispersant was added, and other conditions remained unchanged.

[0139] Comparative Example 9

[0140] Comparative Example 9 Compared with Example 1, in the process of preparing zirconium oxide powder in Comparative Example 9, yttrium oxide is not added, and other conditions remain unchanged.

[0141] Comparative Example 10

[0142] Comparative Example 10 Compared with Example 1, in the process of preparing zirconium oxide powder in Comparative Example 10, calcium oxide and yttrium oxide are not added, and other conditions remain unchanged.

[0143] 0.48 g of the samples prepared in Examples 1-4 and Comparative Examples 1-10 were weighed and poured into a prefabricated cylindrical mold with an inner diameter of 15 mm, and pressed at 20-30 MPa for 1 min on a powder tablet press to form a disc, which was then placed in a closed space, vacuum-sealed, and statically pressed at 200 MPa for 1 min. The obtained disc was then placed in a high-temperature sintering furnace for calcination from room temperature to 1250° C., kept warm for 30 min, then heated to 1400° C., kept warm for 2 h, and then cooled to room temperature. The calcined disc was ground and polished. The thickness of the disc was 0.50 mm. The disc was measured using a spectrophotometer, so that the light source, the disc, and the spectrophotometer probe were in a straight line. The incident light was adjusted to ensure vertical incidence. The light intensity of the light source (I 0 ), and then measure the intensity of light passing through the disc (I), and calculate the approximate transmittance of the disc. The formula is: T = (I / I 0 )×100%, the transmittance is continuously measured every 10nm in the visible light region of 400-780nm to obtain the visible light integral transmittance of the disc. The measuring spot diameter is 4mm. The corrosion resistance of the sample is tested according to GB / T 10125-2021, and the wear resistance of the sample is tested according to GB∕T 12444-2006. The test results are shown in Table 1:

[0144] Table 1

[0145]

[0146] It can be seen from the test results in Table 1 that the zirconium oxide powder prepared in Examples 1-4 of the present invention has excellent permeability, corrosion resistance and wear resistance. By comparing Comparative Example 1 with Examples 1-4, it can be seen that the addition of 2-chloro-2-oxo-1,3,2-dioxaphospholane can effectively improve the permeability and wear resistance of the zirconium oxide powder; by comparing Comparative Example 2 with Examples 1-4, it can be seen that the addition of 1,8-diazacyclo[5,4,0]undecene-7 can effectively improve the permeability and wear resistance of the zirconium oxide powder; by comparing Comparative Example 3 with Examples 1-4, it can be seen that the addition of cellulose nanocrystals can effectively improve the permeability and wear resistance of the zirconium oxide powder; by comparing Comparative Example 4 with Examples 1-4, it can be seen that the addition of glycidyl methacrylate can effectively improve the permeability of the zirconium oxide powder; by comparing Comparative Example 5 with Examples 1-4, it can be seen that the addition of 2-acrylamide-2-methylacrylic acid can effectively improve the permeability of the zirconium oxide powder. Sulfonic acid can effectively improve the permeability of zirconium oxide powder; by comparing comparative example 6 with examples 1-4, it can be seen that adding thioglycolic acid can effectively improve the permeability of zirconium oxide powder; by comparing comparative example 7 with examples 1-4, it can be seen that adding a modified stabilizer can effectively improve the permeability, corrosion resistance and wear resistance of zirconium oxide powder; by comparing comparative example 8 with examples 1-4, it can be seen that adding a composite dispersant can effectively improve the permeability, corrosion resistance and wear resistance of zirconium oxide powder; by comparing comparative example 9 with examples 1-4, it can be seen that adding yttrium oxide can effectively improve the permeability of zirconium oxide powder; by comparing comparative example 10 with examples 1-4, it can be seen that adding calcium oxide and yttrium trioxide can effectively improve the corrosion resistance of zirconium oxide powder.

[0147] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

[0148] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing ultra-high permeability zirconium oxide powder, characterized in that: The following steps are involved: Step (1): dissolving zirconium oxychloride in distilled water, then adding yttrium oxide, a modified stabilizer and aluminum nitrate, stirring and mixing to obtain a reaction solution A; Step (2): dissolving sodium hydroxide in distilled water, adding a composite dispersant, mixing and stirring to obtain a reaction solution B; Step (3): placing the reaction solution B in a heat-collecting constant temperature heating magnetic stirrer, and then adding the reaction solution A dropwise into the reaction solution B until the reaction is completed; Step (4): the mixed liquid obtained by the reaction is allowed to stand for aging, washed, dried, and ball-milled, and then the sintering aid is mixed evenly in anhydrous ethanol, added to a ball mill, and mixed, and the ball milling is continued, dried, sieved, and calcined to obtain ultra-high permeability zirconium oxide powder; The preparation method of the modified stabilizer comprises the following steps: Q1: Add 2-chloro-2-oxo-1,3,2-dioxaphospholane to triethylamine, then add 3-butyn-1-ol and tetrahydrofuran, and react under ice bath conditions to obtain intermediate product 1; add dichloromethane to a container, then add 1,8-diazacyclo[5,4,0]undecene-7, introduce nitrogen, add intermediate product 1 and N-BOC-ethanolamine, mix well, react at low temperature, add glacial acetic acid dropwise to terminate the reaction, continue stirring, rotary evaporate, precipitate, and dry to obtain intermediate product 2; Q2: Add the intermediate product 2 to a container filled with dichloromethane, stir to dissolve, add dichloromethane and trifluoroacetic acid to a constant pressure dropping funnel, mix well, add dropwise to the container, stir, rotary evaporate, precipitate, and dry to obtain the intermediate product 3; Q3: Ultrasonic dispersion of cellulose nanocrystals in deionized water, then adding 2,2,6,6-tetramethylpiperidinyl oxide and sodium bromide, adjusting the pH, and then dropping sodium hypochlorite solution. After the addition is complete, the pH is adjusted, stirring is continued, methanol is added, stirring is continued, the pH is adjusted, stirring is continued, and then the suspension is centrifuged, the upper liquid is taken out, precipitated, centrifuged, washed, dialyzed, and freeze-dried to obtain intermediate 4; Q4: Add the intermediate product 4 to a container filled with N,N-dimethylformamide, and after ultrasonic dispersion, add 1-(3-dimethylaminopropyl)-3-cyclohexylcarbodiimide to activate the carboxyl group, and then add N-hydroxysuccinimide, continue stirring, dissolve the intermediate product 3 in N,N-dimethylformamide, and slowly add it dropwise to the container. After the reaction is completed, heat to extract N,N-dimethylformamide, precipitate, centrifuge, wash, dialyze, and freeze-dry to obtain a modified stabilizer; The preparation method of the composite dispersant comprises the following steps: S1: adding glycidyl methacrylate to deionized water, heating to reflux, and freeze-drying to obtain 2,3-dihydroxy methacrylate; S2: Add acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid, 2,3-dihydroxymethylacrylate, thioglycolic acid and deionized water into a container, heat, and under nitrogen protection, dropwise add an aqueous solution of ammonium persulfate, control the dropping time, and after the dropping is completed, increase the temperature to react. After the reaction is completed, cool down and adjust the pH to obtain a composite dispersant.

2. The method for preparing ultrahigh permeability zirconium oxide powder according to claim 1, characterized in that: In the step (1), the dosage ratio of zirconium oxychloride, distilled water, yttrium oxide, modified stabilizer and aluminum nitrate is (60-70) g: (1-1.5) L: (2.416-2.484) g: (1.8-2.1) g: (1.8-2.1) g, and the stirring and mixing time is 30-40 minutes.

3. The method for preparing ultrahigh permeability zirconium oxide powder according to claim 1, characterized in that: In the Q1, the molar ratio of 2-chloro-2-oxo-1,3,2-dioxaphospholane and 3-butyn-1-ol is (0.8-1.1): (0.9-1.2), the reaction time is 12-14h, the molar ratio of 1,8-diazacyclo[5,4,0]undecene-7, intermediate 1 and N-BOC-ethanolamine is (3.41-6.82): (8.25-16.50): (1.71-3.42), the low temperature reaction temperature is -10~-15°C, and the reaction time is 30-45mi n, the stirring time is continued for 30-35 minutes, the drying temperature is 25-30°C, and the time is 48-60 hours; in Q2, the amount ratio of the intermediate product 2, dichloromethane, dichloromethane and trifluoroacetic acid in the constant pressure dropping funnel is (1.04-2.08) g: (10-20) mL: (10-20) mL: (3-6) mL, the dropping temperature is -5~-8°C, the dropping time is 30-45 minutes, the stirring time is 12-14 hours, the drying temperature is 25-30°C, and the time is 48-50 hours.

4. The method for preparing ultrahigh permeability zirconium oxide powder according to claim 1, characterized in that: In the Q3, the amount ratio of cellulose nanocrystals, deionized water, 2,2,6,6-tetramethylpiperidinium oxide, sodium bromide, sodium hypochlorite and methanol is (3-6) g: (300-600) mL: (60-120) mg: (1.20-2.40) g: (33.10-66.22) g: (30-60) mL. The pH value is adjusted to 5.6 with 0.5 mol / L sodium hydroxide for the first time, and the time for adding sodium hypochlorite solution is 30-40 min. The pH value is adjusted to 10 with 0.5 mol / L sodium hydroxide for the second time, and the stirring time is 12-14 h, and the stirring time is continued for 1-2 h. The third time, 1 mol / L The pH value is adjusted to 1 with hydrochloric acid, the stirring time is continued for 24-30 hours, and the dialysis time is 72-84 hours; in the Q4, the mass ratio of the intermediate product 4, 1-(3-dimethylaminopropyl)-3-cyclohexylcarbodiimide, N-hydroxysuccinimide, and the intermediate product 3 is (100.1-200.3) mg: (433.3-866.4) mg: (260.7-521.2) mg: (1.42-2.88) g, the carboxyl activation time is 30-40 minutes, the stirring time is continued for 12-14 hours, the reaction temperature is 28-30°C, the time is 24-36 hours, the heating temperature is 65-70°C, and the dialysis time is 72-84 hours.

5. The method for preparing ultrahigh permeability zirconium oxide powder according to claim 1, characterized in that: In the step (2), the dosage ratio of sodium hydroxide, distilled water and composite dispersant is (1.6-2.4) g: (1-1.5) L: (0.032-0.048) g, and the mixing and stirring time is 20-30 min.

6. The method for preparing ultrahigh permeability zirconium oxide powder according to claim 1, characterized in that: In the S1, the dosage ratio of glycidyl methacrylate and deionized water is (4.95-7.43) g: (50-75) mL, the heating reflux temperature is 80-90° C., and the time is 9-10 h. In the S2, the dosage ratio of acrylic acid, 2-acrylamide-2-methylpropanesulfonic acid, 2,3-dihydroxymethylacrylate, thioglycolic acid, deionized water and ammonium persulfate aqueous solution is (7.26-9.44) g: (20.7-26.91) g: (1.6-2.08) g: (1.84-2.39) g: (41-53.3) mL: (5-7.5) mL, heating temperature is 60-70°C, concentration of ammonium persulfate aqueous solution is 0.177 g / mL, dropping time is 20-30 min, heating temperature is 70-80°C, pH is adjusted to 7.0-8.0 with 40wt% sodium hydroxide solution.

7. The method for preparing ultrahigh permeability zirconium oxide powder according to claim 1, characterized in that: In the step (3), the temperature of the heat-collecting constant temperature heating magnetic stirrer is 60-70°C, and the stirring rate is 800-1000 rpm, until the pH value is 8-10, and the reaction is completed.

8. The method for preparing ultrahigh permeability zirconium oxide powder according to claim 1, characterized in that: In the step (4), the aging time is 90-150 min, the drying temperature is 80-90° C., the time is 12-14 h, the sintering aid is a mixture of calcium oxide and yttrium trioxide, the ball milling speed is 300-400 rpm, the ball milling time is 180-240 min, the calcination temperature is 500-700° C., and the calcination time is 4-6 h.

Citation Information

Patent Citations

  • Preparation method of nano-stabilized zirconia powder

    CN104211114B

  • Injection molding zirconium oxide and preparation method for same

    CN103803974A

  • High-light transmittance zirconia sintered body, and preparation method and application thereof

    CN106431395A

  • Preparation method of nano zirconia powder for ceramics

    CN110342931A

  • Light transmissive zirconia sintered body, manufacturing method therefor and application thereof

    JP2018002528A