A modified polypropylene material and preparation method thereof

By introducing a self-made pressure-resistant toughening modifier into polypropylene materials and combining it with mica fillers, the problems of insufficient toughness of polypropylene materials in high-voltage cables and the migration and segregation of voltage stabilizers have been solved, significantly improving the breakdown resistance and stability.

CN118546466BActive Publication Date: 2024-10-29FOSHAN WEIKA PLASTIC TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411026271.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-29
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Polypropylene material has insufficient toughness and high elastic modulus in high-voltage cables, making it difficult to use directly. Moreover, the introduced voltage stabilizer is easy to migrate and segregate at high temperatures, resulting in insufficient puncture resistance.

Method used

A self-made pressure-resistant toughening modifier is used to form a polyamide structure through the amidation reaction of 3-aminobenzoic acid methyl ester and trimesoyl chloride, and then combined with alkyl alcohol to introduce terminal alkyl chains for use in modified polypropylene materials. , breaks the regularity of the macromolecular chain of the polypropylene matrix, promotes the formation of β-phase crystals, and disperses them in the mica filler to enhance the anti-breakthrough performance.

Benefits of technology

It improves the toughness and high-temperature voltage breakdown performance of polypropylene materials. Multiple large conjugated π bonds in the molecule capture electrons and hinder electron migration. It is significantly better than the breakdown field strength of traditional voltage stabilizers and has better stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to a modified polypropylene material and a preparation method thereof, and belongs to the technical field of polypropylene composite materials. The modified polypropylene material comprises, by weight, 80-100 parts of copolymerized polypropylene, 30-40 parts of homopolymerized polypropylene, 12-16 parts of oleophilic fillers, 5.5-5 parts of a pressure-resistant toughening modifier, 0.2-0.3 parts of an anti-aging agent and 1.4-1.8 parts of a processing aid. The pressure-resistant toughening modifier is prepared by amidation reaction of methyl 3-aminobenzoate and trimesoyl chloride to form a compound having a multi-amide structure, i.e., an intermediate, and then an alkyl alcohol is subjected to alcoholysis of a terminal methyl ester of the intermediate to introduce a terminal alkyl chain for modification. By introducing and compounding the self-made pressure-resistant toughening modifier, the polypropylene material is endowed with good toughness and high-temperature voltage breakdown resistance, and has broad application value in high-voltage cables.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polypropylene composite materials, and in particular relates to a modified polypropylene material and a preparation method thereof. Background Art

[0002] Polypropylene (PP) is a thermoplastic material that is heat-resistant, corrosion-resistant, and has good electrical insulation properties. Its long-term operating temperature can be stabilized at around 120°C, and it can be widely used in the insulation of various electrical equipment. The polypropylene material itself has a low density, low molding difficulty, and high tensile strength, and is widely used in cable materials.

[0003] However, polypropylene has insufficient toughness and a high elastic modulus, making it difficult to directly use it in the processing of high-voltage cables. While ensuring the excellent electrical properties and stable physical and chemical properties of polypropylene, a method of blending and modification is currently a widely used engineering idea to make up for its shortcomings. Among them, POE (ethylene-octene copolymer) is an elastomer commonly used in engineering. It has good dispersibility for PP and is often used in the blending modification of AC polypropylene cables. However, its melting point is generally low, usually around 50°C, while the operating temperature of high-voltage DC cables usually reaches 60°C. This leads to a decrease in the crystallinity of the composite material when the PP / POE blend is working, a larger carrier free path, and a large amount of space charge injected and accumulated in the PP / POE blend, which will make the material more susceptible to breakdown and reduce the life of the material. The introduction of a certain voltage stabilizer and the use of its ability to capture electrons to inhibit the migration of charges can improve the composite material's anti-breakdown ability to a certain extent. However, commonly used voltage stabilizers are mostly small molecule compounds, which are easy to migrate and segregate during processing and cooling and under high temperature conditions, resulting in insufficient anti-breakdown performance. Excessive introduction of voltage stabilizers will form defects inside the matrix, which will sharply deteriorate the mechanical properties of the material. Summary of the invention

[0004] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a modified polypropylene material and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A modified polypropylene material, comprising, by weight:

[0007] 80-100 parts of copolymer polypropylene, 30-40 parts of homopolymer polypropylene, 12-16 parts of oleophilic filler, 5.5-5 parts of pressure-resistant toughening modifier, 0.2-0.3 parts of anti-aging agent and 1.4-1.8 parts of processing aid.

[0008] A preparation method of a modified polypropylene material comprises the following steps: adding various raw materials into a high-speed mixer and mixing them uniformly; transferring them into a torque rheometer and kneading them at 165-175°C until the torque is stable; then discharging the materials, cooling them, and pelletizing them to obtain the modified polypropylene material.

[0009] Furthermore, the oleophilic filler is selected from oleophilic modified mica powder, and the fineness is not less than 325 mesh.

[0010] Furthermore, the anti-aging agent is compounded by antioxidant 1010, antioxidant 168 and ultraviolet absorber UV531.

[0011] Furthermore, the processing aid is selected from polypropylene wax.

[0012] Wherein, the pressure-resistant toughening modifier is prepared by the following method:

[0013] Step A1: methyl 3-aminobenzoate, triethylamine and anhydrous acetone are mixed, dry nitrogen is introduced for protection, the temperature is controlled to be no higher than 20° C. in an ice-water bath, trimesoyl chloride is added, stirred and reacted for 1.5-2 h, then the temperature is raised to reflux for 0.5-0.8 h, and after the reaction is completed, acetone is recovered by rotary evaporation, the substrate is washed with water, the aqueous phase is removed and vacuum dried to obtain an intermediate;

[0014] Further, the dosage ratio of methyl 3-aminobenzoate, trimesoyl chloride, triethylamine and anhydrous acetone is 0.1 mol: 25-30 mmol: 1-1.5 mL: 30-40 mL, and the amino group in methyl 3-aminobenzoate reacts with the active acyl chloride of trimesoyl chloride to form an amide compound, and the reaction process can be expressed as follows:

[0015]

[0016] Step A2: The intermediate, alkyl alcohol and anhydrous toluene are mixed, nitrogen is introduced for protection, the temperature is raised to 65-80°C, sodium methoxide is added intermittently and stirred for reaction, and the total reaction time of sodium methoxide addition is controlled to be 2.2-3.5h. After the reaction is completed, toluene is recovered by vacuum rotary evaporation, the substrate is washed with water, the water phase is removed and vacuum drying is performed to obtain a pressure-resistant toughening modifier;

[0017] Furthermore, the usage ratio of the intermediate, alkyl alcohol, sodium methoxide and anhydrous toluene is 0.1 mol: 0.32-0.35 mol: 1.2-1.8 g: 60-80 mL, the alkyl alcohol and the methyl ester of the intermediate are alcoholyzed to introduce terminal alkyl chain modification, and the reaction process can be expressed as follows:

[0018]

[0019] Furthermore, the alkyl chain length of the alkyl alcohol is C8-C12, and the alkyl chain of this length has good compatibility and dispersibility with the polypropylene matrix.

[0020] Beneficial effects of the present invention:

[0021] The invention discloses a blended modified polypropylene material. The copolymerized polypropylene and the homopolymerized polypropylene are used as the matrix. A self-made pressure-resistant toughening modifier is introduced to compound the material, so that the polypropylene material has good toughness and high-temperature voltage breakdown resistance performance. The material has broad application value in high-voltage cables. The pressure-resistant toughening modifier is prepared by amidation reaction of 3-aminobenzoic acid methyl ester and trimesoyl chloride to form a compound with a multiamide structure, i.e., an intermediate. Then, an alkyl alcohol and the terminal methyl ester of the intermediate are alcoholyzed to introduce a terminal alkyl chain for modification. In the blended composite system, the terminal long-chain alkyl ester structure of the pressure-resistant toughening modifier has good compatibility with the polypropylene matrix and is easy to be dispersed in the polypropylene matrix, more precisely, it is easier to be dispersed between the polypropylene matrix between the mica fillers, which breaks the regularity of the macromolecular chain of the polypropylene matrix. On the other hand, the multi-branched amide structure in the middle of the molecule promotes the formation of β-phase crystals in polypropylene, which has good toughness and plays a certain role in inducing toughening. Mica has excellent insulation properties, and the dispersed mica particles form a large number of deep traps in the matrix, which increases the migration path of electrons and hinders the breakdown of the matrix. The molecules of the voltage-resistant toughening modifier dispersed between the mica particles contain multi-branched conjugated large π bonds, which have a capturing effect on electrons, capture electrons in the electron migration channel, and enhance the anti-breakdown performance of the matrix. Compared with traditional aromatic voltage stabilizers, the voltage-resistant toughening modifier molecules are multi-branched structures, which are not easy to migrate and segregate in the matrix at high temperatures, and have better stability. In the test, the breakdown field strength at a high temperature of 60°C is significantly better than that of the comparative example of the externally doped voltage stabilizer. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1, preparation of modified polypropylene material, the specific implementation process is as follows:

[0024] 1) Preparation of compressive toughening modifier

[0025] 1.1. Take methyl 3-aminobenzoate, triethylamine and anhydrous acetone, mix them, introduce dry nitrogen for protection, control the temperature of the reaction system at 15±5°C in an ice-water bath, add trimesoyl chloride, stir and react at 150rpm for 1.5h, then raise the temperature to 58±2°C and reflux for 0.5h, wherein the amount ratio of methyl 3-aminobenzoate, trimesoyl chloride, triethylamine and anhydrous acetone is 0.1mol:30mmol:1.5mL:40mL. After the reaction, recover acetone by rotary evaporation, wash the substrate with water, remove the aqueous phase and dry in vacuo to obtain an intermediate.

[0026] 1.2. Take the intermediate, alkyl alcohol and anhydrous toluene and mix them. During the implementation process, the alkyl alcohol is selected from n-octanol with an alkyl chain length of C8. Nitrogen protection is introduced, the temperature is raised to 65°C, and stirring is applied at 60rpm. Take equal amounts of sodium methoxide and divide them into three parts. Feed them with an interval of 30 minutes. After all the sodium methoxide is added, continue to stir and react at a constant temperature. The total reaction time of sodium methoxide is controlled to be 3.5 hours. Among them, the amount ratio of the intermediate, alkyl alcohol, sodium methoxide and anhydrous toluene is 0.1 mol: 0.32 mol: 1.2 g: 60 mL. After the reaction is completed, the toluene is recovered by vacuum rotary evaporation, the substrate is washed with water, the aqueous phase is removed and it is vacuum dried to obtain a pressure-resistant toughening modifier.

[0027] 2) Preparation of blended modified polypropylene

[0028] 2.1. Ingredients in parts by weight: 80 parts of copolymer polypropylene, 4101 type raw material of Sinopec Yanshan Petrochemical Company was used in the implementation process; 35 parts of homopolypropylene, 2401 type raw material of Sinopec Yanshan Petrochemical Company was used in the implementation process; 12 parts of oleophilic filler, Miapeal MS-10 oleophilic modified mica powder of Jiangxi Liankai Chemical Co., Ltd. was used in the implementation process, and the particle size was about 25 μm; 3.5 parts of compressive toughening modifier, which was homemade in this embodiment; 0.2 parts of anti-aging agent, which was pre-mixed and compounded with antioxidant 1010, antioxidant 168 and ultraviolet absorber UV531 in a mass ratio of 1:1:0.15 during the implementation process; 1.6 parts of processing aid, TW-F2053 type polypropylene wax of Jiangsu Tianwen New Material Technology Co., Ltd. was used during the implementation process.

[0029] 2.2. Add all raw materials into a high-speed mixer, mix at 800 rpm for 10 min, transfer to a torque rheometer, control the temperature at 165°C and the speed at 45 rpm. The torque tends to be stable after 15 min of mixing. Cool the discharged material and pelletize it to obtain a modified polypropylene material.

[0030] Example 2, preparation of modified polypropylene material, the specific implementation process is as follows:

[0031] 1) Preparation of compressive toughening modifier

[0032] 1.1. Take methyl 3-aminobenzoate, triethylamine and anhydrous acetone, mix them, introduce dry nitrogen for protection, control the temperature of the reaction system at 5±5°C in an ice-water bath, add trimesoyl chloride, stir and react at 120rpm for 2h, then raise the temperature to 58±2°C and reflux for 0.8h, wherein the amount ratio of methyl 3-aminobenzoate, trimesoyl chloride, triethylamine and anhydrous acetone is 0.1mol:25mmol:1mL:30mL. After the reaction, recover acetone by rotary evaporation, wash the substrate with water, remove the aqueous phase and dry in vacuo to obtain an intermediate.

[0033] 1.2. Take the intermediate, alkyl alcohol and anhydrous toluene and mix them. During the implementation process, the alkyl alcohol is selected from n-decanol with an alkyl chain length of C10. Nitrogen protection is introduced, the temperature is raised to 75°C, and stirring is applied at 60rpm. Take equal amounts of sodium methoxide and divide them into three parts. Feed them with an interval of 25 minutes. After all the sodium methoxide is added, continue to stir and react at a constant temperature. The total reaction time of sodium methoxide is controlled to be 3 hours. Among them, the amount ratio of the intermediate, alkyl alcohol, sodium methoxide and anhydrous toluene is 0.1 mol: 0.33 mol: 1.5 g: 70 mL. After the reaction is completed, the toluene is recovered by vacuum rotary evaporation, the substrate is washed with water, the aqueous phase is removed and it is vacuum dried to obtain a pressure-resistant toughening modifier.

[0034] 2) Preparation of blended modified polypropylene

[0035] 2.1. Ingredients in parts by weight: 90 parts of copolymer polypropylene, 4101 type raw material of Sinopec Yanshan Petrochemical Company was used in the implementation process; 30 parts of homopolypropylene, 2401 type raw material of Sinopec Yanshan Petrochemical Company was used in the implementation process; 13 parts of oleophilic filler, Miapeal MS-10 oleophilic modified mica powder of Jiangxi Liankai Chemical Co., Ltd. was used in the implementation process, and the particle size was about 25 μm; 4.5 parts of compressive toughening modifier, which was homemade in this embodiment; 0.2 parts of anti-aging agent, which was pre-mixed and compounded with antioxidant 1010, antioxidant 168 and ultraviolet absorber UV531 in a mass ratio of 1:1:0.15 during the implementation process; 1.4 parts of processing aid, TW-F2053 type polypropylene wax of Jiangsu Tianwen New Material Technology Co., Ltd. was used during the implementation process.

[0036] 2.2. Add all raw materials into a high-speed mixer, mix at 800 rpm for 10 min, transfer to a torque rheometer, control the temperature at 170°C and the speed at 45 rpm. The torque tends to be stable after 16 min of mixing. Cool the discharged material and pelletize it to obtain a modified polypropylene material.

[0037] Example 3, preparation of modified polypropylene material, the specific implementation process is as follows:

[0038] 1) Preparation of compressive toughening modifier

[0039] 1.1. Take methyl 3-aminobenzoate, triethylamine and anhydrous acetone, mix them, introduce dry nitrogen for protection, control the temperature of the reaction system at 5±5°C in an ice-water bath, add trimesoyl chloride, stir and react at 150rpm for 1.7h, then raise the temperature to 58±2°C and reflux for 0.6h, wherein the amount ratio of methyl 3-aminobenzoate, trimesoyl chloride, triethylamine and anhydrous acetone is 0.1mol:28mmol:1.2mL:40mL. After the reaction, recover acetone by rotary evaporation, wash the substrate with water, remove the aqueous phase and dry in vacuo to obtain an intermediate.

[0040] 1.2. Take the intermediate, alkyl alcohol and anhydrous toluene and mix them. During the implementation process, the alkyl alcohol is selected from n-dodecanol with an alkyl chain length of C12. Nitrogen protection is introduced, the temperature is raised to 80°C, and stirring is applied at 90rpm. Take equal amounts of sodium methoxide and divide them into three parts. Feed them with an interval of 20 minutes. After all the sodium methoxide is added, continue to stir and react at a constant temperature. The total reaction time of sodium methoxide is controlled to be 2.2 hours. Among them, the amount ratio of the intermediate, alkyl alcohol, sodium methoxide and anhydrous toluene is 0.1 mol: 0.35 mol: 1.8 g: 80 mL. After the reaction is completed, the toluene is recovered by vacuum rotary evaporation, the substrate is washed with water, the aqueous phase is removed and it is vacuum dried to obtain a pressure-resistant toughening modifier.

[0041] 2) Preparation of blended modified polypropylene

[0042] 2.1. Ingredients in parts by weight: 100 parts of copolymer polypropylene, using 4101 raw material from Sinopec Yanshan Petrochemical Company during the implementation process; 40 parts of homopolypropylene, using 2401 raw material from Sinopec Yanshan Petrochemical Company during the implementation process; 16 parts of oleophilic filler, using Miapeal MS-10 oleophilic modified mica powder from Jiangxi Liankai Chemical Co., Ltd. during the implementation process, with a particle size of about 25 μm; 5 parts of compressive toughening modifier, which is homemade in this embodiment; 0.3 parts of aging resistance agent, using antioxidant 1010, antioxidant 168 and ultraviolet absorber UV531 pre-mixed and compounded in a mass ratio of 1:1:0.15 during the implementation process; 1.8 parts of processing aid, using TW-F2053 polypropylene wax from Jiangsu Tianwen New Material Technology Co., Ltd. during the implementation process.

[0043] 2.2. Add all raw materials into a high-speed mixer, mix at 800 rpm for 10 min, transfer to a torque rheometer, control the temperature at 175°C and the speed at 45 rpm. The torque tends to be stable after 18 min of mixing. Cool the discharged material and pelletize it to obtain a modified polypropylene material.

[0044] Example 4, preparation of modified polypropylene material, the specific implementation process is as follows:

[0045] 1) Preparation of compressive toughening modifier

[0046] 1.1. Take methyl 3-aminobenzoate, triethylamine and anhydrous acetone, mix them, introduce dry nitrogen for protection, control the temperature of the reaction system at 10±5°C in an ice-water bath, add trimesoyl chloride, stir and react at 150rpm for 1.8h, then raise the temperature to 58±2°C and reflux for 0.7h, wherein the amount ratio of methyl 3-aminobenzoate, trimesoyl chloride, triethylamine and anhydrous acetone is 0.1mol:28mmol:1.5mL:40mL. After the reaction, recover acetone by rotary evaporation, wash the substrate with water, remove the aqueous phase and dry in vacuo to obtain an intermediate.

[0047] 1.2. Take the intermediate, alkyl alcohol and anhydrous toluene and mix them. During the implementation process, the alkyl alcohol is selected from undecanol with an alkyl chain length of C11. Nitrogen protection is introduced, the temperature is raised to 75°C, and stirring is applied at 90rpm. Take equal amounts of sodium methoxide and divide them into three parts. Feed them with an interval of 30 minutes. After all the sodium methoxide is added, continue to stir and react at a constant temperature. The total reaction time of sodium methoxide is controlled to be 3.2 hours. Among them, the amount ratio of the intermediate, alkyl alcohol, sodium methoxide and anhydrous toluene is 0.1 mol: 0.34 mol: 1.6 g: 75 mL. After the reaction is completed, the toluene is recovered by vacuum rotary evaporation, the substrate is washed with water, the aqueous phase is removed and it is vacuum dried to obtain a pressure-resistant toughening modifier.

[0048] 2) Preparation of blended modified polypropylene

[0049] 2.1. Ingredients in parts by weight: 92 parts of copolymer polypropylene, 4101 type raw material of Sinopec Yanshan Petrochemical Company was used in the implementation process; 36 parts of homopolypropylene, 2401 type raw material of Sinopec Yanshan Petrochemical Company was used in the implementation process; 15 parts of oleophilic filler, Miapeal MS-10 oleophilic modified mica powder of Jiangxi Liankai Chemical Co., Ltd. was used in the implementation process, and the particle size was about 25 μm; 4.2 parts of compressive toughening modifier, which was homemade in this embodiment; 0.2 parts of anti-aging agent, which was pre-mixed and compounded with antioxidant 1010, antioxidant 168 and ultraviolet absorber UV531 in a mass ratio of 1:1:0.15 during the implementation process; 1.6 parts of processing aid, TW-F2053 type polypropylene wax of Jiangsu Tianwen New Material Technology Co., Ltd. was used during the implementation process.

[0050] 2.2. Add all raw materials into a high-speed mixer, mix at 800 rpm for 10 min, transfer to a torque rheometer, control the temperature at 170°C and the speed at 45 rpm. The torque tends to be stable after 18 min of mixing. Cool the discharged material and pelletize it to obtain a modified polypropylene material.

[0051] In the comparative example, POE resin and voltage stabilizer are selected to replace the pressure-resistant toughening modifier, and the polypropylene material is prepared by blending and modification. The specific implementation process is as follows:

[0052] Ingredients: 95 parts of copolymerized polypropylene, 4101 type raw material of Sinopec Yanshan Petrochemical Company was used in the implementation process; 35 parts of homopolymerized polypropylene, 2401 type raw material of Sinopec Yanshan Petrochemical Company was used in the implementation process; 15 parts of oleophilic filler, Miapeal MS-10 oleophilic modified mica powder of Jiangxi Liankai Chemical Co., Ltd. was used in the implementation process, and the particle size was about 25 μm; 8 parts of POE resin, EPF31HR type raw material of North Huajin Chemical Industry Group Co., Ltd. was used in the implementation process; 1.5 parts of voltage stabilizer, industrial grade 4-propyleneoxy-2-hydroxybenzophenone was used in the implementation process; 0.2 parts of aging agent, antioxidant 1010, antioxidant 168 and ultraviolet absorber UV531 were pre-mixed and compounded in a mass ratio of 1:1:0.15 in the implementation process; 1.6 parts of processing aid, TW-F2053 type polypropylene wax of Jiangsu Tianwen New Material Technology Co., Ltd. was used in the implementation process; the specific blending process is the same as Example 4.

[0053] The modified polypropylene material was plasticized and extruded by a twin-screw extruder, wherein the temperature zones of the twin-screw extruder were set to 170°C, 180°C, 200°C, 220°C, 200°C, and 190°C, and the die temperature was 205°C. The melt was extruded into a flat die, the die temperature was 80°C, the pressure was 3.0MPa, the pressure was maintained for 180s, and the sheet was cooled to form a sheet. Samples were taken from the sheet for testing, including: tensile testing with reference to GB / T 1040.2-2006, with a tensile rate of 100mm / min; impact performance testing with reference to GB / T 1843-2008 standard, with a test temperature of 23°C; pressure resistance testing with reference to GB / T1408.1-2016 standard, and the sample was balanced in a constant temperature box at a temperature of 60°C and a humidity of 70% for 24h before testing; the specific test results are shown in Table 1:

[0054] Table 1

[0055]

[0056] It can be seen from the test results in Table 1 that the modified polypropylene material prepared in the embodiment has good toughness, especially the breakdown strength is significantly better than that of the comparative example.

[0057] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0058] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A modified polypropylene material, characterized in that: The composition comprises, by weight: 80-100 parts of copolymerized polypropylene, 30-40 parts of homopolymerized polypropylene, 12-16 parts of oleophilic filler, 5.5-5 parts of compressive toughening modifier, 0.2-0.3 parts of anti-aging agent and 1.4-1.8 parts of processing aid; The pressure-resistant toughening modifier is prepared by the following method: Step A1: methyl 3-aminobenzoate, triethylamine, and anhydrous acetone are mixed, and dry nitrogen is introduced for protection. The temperature is controlled at no higher than 20°C in an ice-water bath. Trimesoyl chloride is added, and the reaction is stirred for 1.5-2 hours. The temperature is then raised to reflux for 0.5-0.8 hours. After the reaction is completed, the acetone is recovered by rotary evaporation. The substrate is washed with water, the aqueous phase is removed, and the product is dried under vacuum to obtain an intermediate. The ratio of methyl 3-aminobenzoate, trimesoyl chloride, triethylamine, and anhydrous acetone is 0.1 mol: 25-30 mmol: 1-1.5 mL: 30-40 mL. Step A2: The intermediate, alkyl alcohol, and anhydrous toluene are mixed, nitrogen is introduced, the temperature is raised to 65-80°C, sodium methoxide is intermittently added, and the reaction is stirred. The total reaction time of the sodium methoxide addition is controlled to be 2.2-3.5 hours. After the reaction is completed, the toluene is recovered by vacuum rotary evaporation, the substrate is washed with water, the aqueous phase is removed, and the product is vacuum dried to obtain a pressure-resistant toughening modifier, wherein the amount ratio of the intermediate, alkyl alcohol, sodium methoxide, and anhydrous toluene is 0.1 mol: 0.32-0.35 mol: 1.2-1.8 g: 60-80 mL, and the alkyl chain length of the alkyl alcohol is C8-C12; The oleophilic filler is oleophilic modified mica powder with a fineness of not less than 325 meshes.

2. A modified polypropylene material according to claim 1, characterized in that: The anti-aging agent is compounded by antioxidant 1010, antioxidant 168 and ultraviolet absorber UV531.

3. A modified polypropylene material according to claim 1, characterized in that: The processing aid is polypropylene wax.

4. The method for preparing a modified polypropylene material according to any one of claims 1 to 3, characterized in that: The specific method is as follows: adding each raw material into a high-speed mixer and mixing evenly, transferring the raw material into a torque rheometer and kneading at 165-175° C. until the torque is stable, then discharging the material, cooling and pelletizing to obtain a modified polypropylene material.

Citation Information

Patent Citations

  • Organic crystallization nucleating agent and preparation method and application thereof

    CN102786716A

  • Production method for amide nucleating agent

    CN104211612A