Resin coated sand and preparation method thereof
By combining phenolic resin, coupling agent and quartz sand, and dispersing, vibrating screen and vibrating air-cooled bed, the problem of insufficient bonding of coated sand is solved, and its sand resistance and resistance in oil and gas wells is improved The crushing ability ensures long-term stable contact and flow diversion capabilities.
Patent Information
- Application Number
- CN202411016786.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-29
AI Technical Summary
The existing coated sand has weak bonding and is prone to breaking, which affects its sandproof effect in oil and gas wells.
Phenolic resin and coupling agent (polyvinylpyrrolidone, cetyltrimethylammonium bromide, isopropyltristitanate, isopropyldisstearoyloxy aluminate, γ-urea The combination of ylpropyltriethoxysilane and quartz sand is enhanced by dispersion, vibration screen and vibration air-cooled bed processing to enhance the degree of bonding and anti-breaking ability.
It improves the durability and anti-broken ability of coated sand, ensures its stable contact in oil and gas wells for a long time, prevents crushing, maintains flow diversion capacity, and extends service life.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention is applicable to the technical field of sand prevention of oil, water and gas wells, and provides resin-coated sand and a preparation method thereof. Background Art
[0002] Problems such as proppant spitting back and formation sand production after oil and gas well fracturing have always restricted the normal performance of oil well production capacity. In mild cases, they can affect the normal production of oil and gas wells, and in severe cases, they can lead to the scrapping of oil and gas wells.
[0003] In the existing sand control technology, coated sand is usually used. Coated sand is a sand-like material coated on the surface of the substrate through a specific process. It is usually used to increase the surface hardness, wear resistance, corrosion resistance or other special properties of the substrate.
[0004] In the prior art, the coated sand prepared by the conventional method for preparing coated sand has a weak bonding degree and is easily broken, which affects the use. Summary of the invention
[0005] In view of the above-mentioned defects, the object of the present invention is to provide a resin-coated sand and a preparation method thereof, in order to solve the problems in the background.
[0006] A resin-coated sand comprises quartz sand, wherein the quartz sand is coated with phenolic resin and a coupling agent, wherein the phenolic resin comprises phenolic resin powder and phenolic resin liquid, and the coupling agent comprises polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyloxyaluminate, and γ-ureidopropyl triethoxysilane.
[0007] Furthermore, the weight ratio of the quartz sand, phenolic resin and coupling agent is 8.8-9.2:0.6-0.8:0.22-0.28.
[0008] Furthermore, the weight ratio of polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyloxyaluminate, and γ-ureidopropyl triethoxysilane is 0.2-1.8: 0.2-1.8: 0.2-1: 0.2-1.8: 0.2-1.8.
[0009] A method for preparing resin-coated sand comprises the following steps:
[0010] Step 1: Pour high-purity quartz sand into the raw sand quantitative device through a bucket elevator and weigh it;
[0011] Step 2: Add quartz sand into the sand mixer, and add coupling agent and phenolic resin in sequence during the mixing process of the sand mixer, and stir evenly;
[0012] Step 3: After mixing, it passes through a belt conveyor and enters a dispersing machine for dispersing;
[0013] Step 4: The broken materials enter the vibrating screen;
[0014] Step 5: The screened material passes through a vibrating air-cooling bed;
[0015] Step 6: Get the resin coated sand.
[0016] Furthermore, the weight ratio of the phenolic resin powder to the phenolic resin liquid is 0.7-1.4:3.6-4.3.
[0017] Furthermore, the particle size of the resin coated sand is 0.3-1.4 mm, and the density of the resin coated sand is 1.3-1.6 t / m 3 .
[0018] Furthermore, there are two dispersing machines, and the speed of the dispersing machine is 50r / min, and the volume is 0.5m 3 .
[0019] Furthermore, there are two vibrating screens, and the vibration frequency of the vibrating screens is 50 Hz, and the vibration intensity is 0-5000.
[0020] Furthermore, there are two vibrating air-cooling beds, and the vibration frequency of the vibrating air-cooling beds is 50 Hz, and the vibration intensity is 0-30000.
[0021] Beneficial Effects
[0022] The present invention enhances the bonding degree between quartz sand and phenolic resin powder through the synergistic effect of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, triisostearoyl isopropyl titanate, isopropyl distearoyloxyaluminate, and γ-ureidopropyl triethoxysilane; the phenolic resin powder can bond quartz sand particles together to prevent them from falling off during the production process, thereby improving the performance and durability of the coated sand. The phenolic resin liquid coated on the surface of the sand particles can change the original point-to-point contact between the sand particles into a small area contact, thereby reducing the load acting on the sand particles and increasing the anti-crushing ability of the sand particles.
[0023] The disperser makes it easier to mix the crushed sand particles evenly with other raw materials, thereby improving the overall performance of the resin coated sand; the dispersed coating sand is sent to the vibrating screen to remove impurities and unqualified particles in the coating sand, further improving the purity and quality stability of the product; the vibrating air-cooling bed adjusts the gaps between the coating sand particles and improves fluidity.
[0024] When the coated sand is applied to oil and gas wells for sand prevention, the coated sand can be in contact with the reservoir rock for a long time and has a strong bonding degree, taking into account the basic function of conventional proppants to support diversion fractures, while preventing the coated sand from being crushed, reducing the load on the sand particles, and will not be destroyed by fracturing construction, so that the oil displacement agent and the core are in contact at the reservoir depth; the raw materials are easy to obtain and the preparation process is simple. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0026] Example:
[0027] A resin-coated sand comprises phenolic resin, quartz sand and a coupling agent, wherein the weight ratio of quartz sand, phenolic resin and coupling agent is 8.8-9.2:0.6-0.8:0.22-0.28; the coupling agent comprises polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyloxyaluminate and γ-ureidopropyl triethoxysilane.
[0028] A method for preparing resin-coated sand comprises the following steps:
[0029] Step 1: Pour high-purity quartz sand into the raw sand quantitative device through a bucket elevator and weigh it;
[0030] Step 2: Add quartz sand to the sand mixer, and add coupling agent, phenolic resin powder, and phenolic resin liquid in the mixing process of the sand mixer in turn, and stir evenly; the coupling agent is composed of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, triisostearoyl isopropyl titanate, isopropyl distearyloxyaluminate, and γ-ureidopropyl triethoxysilane. The good adhesion and film-forming properties of polyvinyl pyrrolidone enable it to form a stable interface between quartz sand and phenolic resin, thereby improving the overall performance of the material. Hexadecyl trimethyl ammonium bromide interacts with the surface of quartz sand through its surface charge and functional groups, thereby enhancing the interfacial bonding force between quartz sand and phenolic resin. Triisostearoyl isopropyl titanate produces chemical bonding at the interface between inorganic powder and matrix resin to form a monomolecular film, which can significantly improve the compatibility between inorganic fillers and organic matrices. Isopropyl distearyloxyaluminate contains a group that can react with active hydrogen, and can form a bond with an inorganic filler, thereby improving the affinity and bonding force between quartz sand and phenolic resin, producing an anti-settling effect, and increasing the bonding strength. γ-ureidopropyl triethoxysilane can significantly enhance the bonding between the two materials by chemically bonding (coupling) the phenolic resin and quartz sand. The weight ratio of polyvinyl pyrrolidone, hexadecyl trimethylammonium bromide, triisostearoyl titanate isopropyl, isopropyl distearyloxyaluminate, and γ-ureidopropyl triethoxysilane is 0.2-1.8: 0.2-1.8: 0.2-1: 0.2-1.8: 0.2-1.8. The synergistic effect of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane enhances the bonding between quartz sand and phenolic resin powder. Phenolic resin powder can bond quartz sand particles together to prevent them from falling off during the production process, thereby improving the performance and durability of the coated sand. The phenolic resin liquid coated on the surface of the sand particles can change the original point-to-point contact between the sand particles into a small area contact, reducing the load on the sand particles and increasing the sand particles' ability to resist crushing.
[0031] Step 3: After mixing, the mixture enters the dispersing machine through the belt conveyor for dispersing; there are two dispersing machines, and the speed of the dispersing machine is 50r / min, and the volume is 0.5m 3 .
[0032] Step 4: The broken materials enter the vibrating screen with a screening hole of 0.3-1.4mm; there are two vibrating screens, and the vibration frequency of the vibrating screens is 50Hz, and the vibration intensity is 0-5000.
[0033] Step 5: The screened material passes through a vibrating air-cooling bed, where the material is suspended in the fluidized bed through vibration, and is cooled by cold air to reduce the material temperature; there are two vibrating air-cooling beds, and the vibration frequency of the vibrating air-cooling beds is 50Hz, and the vibration intensity is 0-30000.
[0034] Step 6: Obtain resin-coated sand and measure and package it.
[0035] Phenolic resin has excellent heat resistance and chemical resistance, can maintain stability in high temperature and chemical corrosion environment, and has good mechanical strength and rigidity. The phenolic resin solution is applied to the surface of quartz sand through a sand mixer. When the phenolic resin dries on the surface of quartz sand, the phenolic resin will form a protective film on the surface of quartz sand, enhancing the corrosion resistance, wear resistance and structural strength of quartz sand. Although phenolic resin has a certain bonding ability, its bonding ability decreases after drying. For this reason, this scheme introduces a coupling agent.
[0036] In this scheme, the concentration of phenolic resin in the phenolic resin solution is not less than 70%.
[0037] Coupling agents can form chemical bonds or physical adsorption at the interface of two or more different materials (such as organic and inorganic substances), thereby significantly improving the bonding strength between them. This enhanced bonding strength helps to reduce the separation or peeling phenomenon between materials and improve the mechanical properties of the overall material. In addition, coupling agents can reduce the degradation rate of materials under environmental conditions (such as moisture, high temperature or chemical media). By forming a protective coating or interface structure on the surface of the material, coupling agents help to enhance the weather resistance and chemical resistance of the material. Through the dual effects of coupling agents and phenolic resins, the mechanical properties of quartz sand are further improved and its supporting capacity is increased.
[0038] Since the coupling agent and phenolic resin easily cause high-purity quartz sand to stick together to form agglomerates, the agglomerate quartz sand is difficult to be transported to the cracks of the oil well.
[0039] The preliminary mixed materials need to be sent to the disintegrator to be broken into granular materials. During the production process of resin-coated sand, the sand particles may clump together due to the adhesion of the resin and other factors. These lumps not only affect the uniformity and quality of the product, but may also cause obstacles to the subsequent production process. The disintegrator can effectively break these lumps into individual sand particles to ensure the uniformity and consistency of the resin-coated sand. Through the processing of the disintegrator, the workload of manual breaking of lumps can be reduced and production efficiency can be improved. At the same time, due to the high degree of automation of the disintegrator, the impact of human factors on product quality can be reduced. The broken sand particles are easier to mix evenly with other raw materials, thereby improving the overall performance of the resin-coated sand. This includes improving the strength, hardness, wear resistance and other indicators of the product.
[0040] The dispersed coating sand is sent to the vibrating screen. The main function of the disperser is to disperse the large particles or agglomerated coating sand into smaller particles. This helps to eliminate the unevenness in the material and make the particle size distribution of the coating sand more uniform. After the disperser breaks the large particles into small particles, it reduces the clogging of the material on the screen. This helps to improve the screening efficiency of the vibrating screen, reduce energy consumption, and reduce the wear and replacement frequency of the screen. The vibrating screen is the process of separating the dispersed coating sand according to the particle size. Through the screening effect of the screen, the coating sand of different particle sizes can be separated to meet the requirements of the subsequent process for the particle size of the material. The particle size distribution of the coating sand after being processed by the disperser is more reasonable, which helps to improve the screening effect. The screened material can better meet the requirements of the subsequent process for particle size, shape, etc. The dispersion and screening processes work together on the coating sand to make its particle size more uniform. This helps to improve the overall quality of the product, including performance indicators such as strength, hardness, and wear resistance. During the screening process, impurities and unqualified particles in the coating sand can also be removed, further improving the purity and quality stability of the product.
[0041] The screened coated sand is sent to the vibrating air cooling bed, where the moisture contained in the granular material is removed during vibration to prevent the subsequent granular material from sticking together again. The vibrating air cooling bed quickly cools the screened coated sand by air cooling. The air cooling system can efficiently remove the heat from the surface of the coated sand, so that it reaches the required temperature range in a short time. The design of the vibrating air cooling bed allows the coated sand to be evenly heated and dissipated during the cooling process, avoiding local overheating or overcooling, and ensuring the overall quality of the coated sand. During the cooling process, the screened coated sand may clump due to the decrease in temperature and increase in humidity. The vibration function of the vibrating air cooling bed can effectively destroy these clumps and keep the coated sand loose. Through the vibration effect, the gaps between the coated sand particles are adjusted and the fluidity is improved. This is very beneficial for subsequent transportation, storage and use. Although the coated sand has been preliminarily screened, the vibrating air cooling bed may produce some fine particles or impurities during the cooling process. Through the action of vibration and airflow, these fine particles or impurities can be further screened out to improve the purity of the coated sand. During the cooling process, the attachments on the surface of the coated sand (such as resin residue, dust, etc.) may become easier to remove. The airflow and vibration of the vibrating air cooling bed help to peel these attachments off the surface of the coated sand and maintain its cleanliness. The vibrating air cooling bed is usually designed as a continuous operation equipment, which can be seamlessly connected with the screening equipment at the front end and the conveying equipment at the back end to form a complete production line. This helps to improve production efficiency and reduce labor costs. Modern vibrating air cooling beds are often equipped with advanced automatic control systems that can monitor and adjust the operating status and parameters of the equipment in real time. This helps to ensure the efficient and stable operation of the equipment and improve production efficiency and product quality.
[0042] First, high-purity quartz sand is mixed with sand-carrying fluid and then pumped to the oil well cracks by a fracturing pump truck, and the high-purity quartz sand is mixed with the original formation to form a mixed sand zone; secondly, the resin-coated sand in step six is pumped to the oil well cracks by a fracturing pump truck, and then the coated sand forms a thin but tough resin layer at the oil well cracks, thereby enhancing the strength and anti-crushing ability of the sand particles and preventing the fracturing sand from spitting out;
[0043] The phenolic resin coating on the outside of the coated sand can change the original proppant into a contact with a certain area, increasing the interaction force between the quartz sand grains; when the coated sand enters the fracture, the phenolic resin layer softens first due to the influence of temperature. In this process, the quartz sand grains are consolidated together due to the polymerization of the phenolic resin to form a mesh filter segment with permeability. After the phenolic resin is cured, the contact between the sand grains changes from point-to-point contact to small-area contact, which reduces the load on the sand grains and increases the anti-crushing ability of the sand grains. The consolidated sand grains can form a stable support structure and effectively prevent the fracturing sand from spitting out. At the same time, since the mesh filter segment formed by the coated sand has a certain permeability, it can maintain the conductivity of the oil layer, which is conducive to the long-term stable production of the oil well. The coated sand takes into account the basic function of conventional proppants to support the diversion fracture, while preventing the coated sand from being crushed, reducing the load on the sand grains, and will not be destroyed by the fracturing construction, so that the oil displacement agent and the core are in contact at the reservoir depth; the raw materials are easy to obtain and the preparation process is simple.
[0044] Embodiment 1:
[0045] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 8.8:0.6:0.22;
[0046] The coupling agent is polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyloxyaluminate, and γ-ureidopropyl triethoxysilane, and the weight ratio of polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyloxyaluminate, and γ-ureidopropyl triethoxysilane is 0.2:1:1:1:1.8.
[0047] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 0.7:3.6. The test results are shown in Table 1 below. Density of resin-coated sand 1.3t / m 3 .
[0048] Table 1 Coated sand parameters
[0049]
[0050] Embodiment 2:
[0051] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 8.9:0.6:0.24;
[0052] The coupling agent is polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyloxyaluminate, and γ-ureidopropyl triethoxysilane, and the weight ratio of polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyloxyaluminate, and γ-ureidopropyl triethoxysilane is 1.8:1:1:1:0.2.
[0053] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 0.7:3.6. The test results are shown in Table 2 below. Density of resin-coated sand 1.3t / m 3 .
[0054] Table 2 Coating sand parameters
[0055]
[0056] Embodiment 3:
[0057] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 9.0:0.7:0.26;
[0058] The coupling agent is polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane, and the weight ratio of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane is: 1:1.8:1:0.2:1.
[0059] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 0.7:3.6. The test results are shown in Table 3 below. Density of resin-coated sand 1.3t / m 3 .
[0060] Table 3 Coating sand parameters
[0061]
[0062] Embodiment 4:
[0063] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 9.1:0.8:0.26;
[0064] The coupling agent is polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane. The weight ratio of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane is 1:0.2:1:1.8:1.
[0065] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 0.7:3.6. The test results are shown in Table 4 below. Density of resin-coated sand 1.4t / m 3 .
[0066] Table 4 Coating sand parameters
[0067]
[0068] Embodiment 5:
[0069] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 9.2:0.8:0.28;
[0070] The coupling agent is polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane. The weight ratio of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane is 1:1.4:0.2:1.4:1.
[0071] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 0.7:3.6. The test results are shown in Table 5 below. Density of resin-coated sand 1.4t / m 3 .
[0072] Table 5 Coating sand parameters
[0073]
[0074] Embodiment 6:
[0075] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 9.0:0.7:0.25;
[0076] The coupling agent is polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane. The weight ratio of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane is 1:1.4:0.2:1.4:1.
[0077] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 0.7:3.6. The test results are shown in Table 6 below. Density of resin-coated sand 1.5t / m 3 .
[0078] Table 6 Coating sand parameters
[0079]
[0080] Embodiment 7:
[0081] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 9.0:0.7:0.25;
[0082] The coupling agent is polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane. The weight ratio of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane is 1:1.4:0.2:1.4:1.
[0083] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 0.9:3.8. The test results are shown in Table 7 below. Density of resin-coated sand 1.5t / m 3 .
[0084] Table 7 Coating sand parameters
[0085]
[0086] Embodiment 8:
[0087] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 9.0:0.7:0.25;
[0088] The coupling agent is polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane. The weight ratio of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane is 1:1.4:0.2:1.4:1.
[0089] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 1:4. The test results are shown in Table 8 below. Density of resin-coated sand 1.6t / m 3 .
[0090] Table 8 Coating sand parameters
[0091]
[0092] Embodiment 9:
[0093] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 9.0:0.7:0.25;
[0094] The coupling agent is polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane. The weight ratio of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane is 1:1.4:0.2:1.4:1.
[0095] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 1.2:4.1. The test results are shown in Table 9 below. Density of resin-coated sand 1.6t / m 3 .
[0096] Table 9 Coating sand parameters
[0097]
[0098] Embodiment 10:
[0099] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 9.0:0.7:0.25;
[0100] The coupling agent is polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane. The weight ratio of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane is 1:1.4:0.2:1.4:1.
[0101] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 1.3:4.2. The test results are shown in Table 10 below. Density of resin-coated sand 1.5t / m 3 .
[0102] Table 10 Coating sand parameters
[0103]
[0104] Embodiment 11:
[0105] By weight, the proportion of quartz sand, phenolic resin and coupling agent is 9.0:0.7:0.25;
[0106] The coupling agent is polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane. The weight ratio of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane is 1:1.4:0.2:1.4:1.
[0107] The phenolic resin includes phenolic resin powder and phenolic resin liquid, and the weight ratio of phenolic resin powder to phenolic resin liquid is 1.4:4.3. The test results are shown in Table 11 below. Density of resin-coated sand 1.5t / m 3 .
[0108] Table 11 Coating sand parameters
[0109]
[0110] In summary, the present invention enhances the bonding degree between quartz sand and phenolic resin powder through the synergistic effect of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane; the phenolic resin powder can bond the quartz sand particles together to prevent them from falling off during the production process, thereby improving the performance and durability of the coated sand. The phenolic resin liquid coated on the surface of the sand particles can change the original point-to-point contact between the sand particles into a small area contact, reducing the load acting on the sand particles and increasing the sand particles' ability to resist crushing.
[0111] When the coated sand is applied to oil and gas wells for sand prevention, the coated sand can be in contact with the reservoir rock for a long time, taking into account the basic function of conventional proppants to support diversion fractures, while preventing the coated sand from being crushed, reducing the load on the sand particles, and will not be destroyed by fracturing construction, so that the oil displacement agent and the core are in contact at the reservoir depth; the raw materials are easy to obtain and the preparation process is simple.
[0112] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing resin-coated sand, comprising the following steps: Step 1: pouring high-purity quartz sand into a raw sand quantitative device through a bucket elevator and weighing it; Step 2: Add quartz sand into the sand mixer, and add coupling agent and phenolic resin in sequence during the mixing process of the sand mixer, and stir evenly; Step 3: After mixing, it passes through a belt conveyor and enters a dispersing machine for dispersing; Step 4: The broken materials enter the vibrating screen; Step 5: The screened material passes through a vibrating air-cooling bed; Step 6: Obtaining resin coated sand; The resin-coated sand comprises quartz sand, the outer surface of which is coated with phenolic resin and a coupling agent, wherein the phenolic resin comprises phenolic resin powder and phenolic resin liquid, and the coupling agent comprises polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate, and γ-ureidopropyl triethoxysilane; The weight ratio of the phenolic resin powder to the phenolic resin liquid is 0.7-1.4:3.6-4.
3.
2. The method for preparing resin-coated sand according to claim 1, characterized in that: The dosage ratio of the quartz sand, phenolic resin and coupling agent is 8.8-9.2:0.6-0.8:0.22-0.28 by weight.
3. The method for preparing resin-coated sand according to claim 1, characterized in that: The weight ratio of the polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, isopropyl triisostearoyl titanate, isopropyl distearoyl aluminate and γ-ureidopropyl triethoxysilane is 0.2-1.8:0.2-1.8:0.2-1:0.2-1.8:0.2-1.
8.
4. The method for preparing resin-coated sand according to claim 1, characterized in that: The particle size of the resin coated sand is 0.3-1.4 mm, and the density of the resin coated sand is 1.3-1.6 t / m 3 .
5. The method for preparing resin-coated sand according to claim 1, characterized in that: There are two dispersing machines, and the speed of the dispersing machine is 50r / min, and the volume is 0.5m 3 .
6. The method for preparing resin-coated sand according to claim 1, characterized in that: There are two vibrating screens, and the vibration frequency of the vibrating screens is 50 Hz, and the vibration intensity is 0-5000.
7. The method for preparing resin-coated sand according to claim 1, characterized in that: There are two vibrating air-cooling beds, and the vibration frequency of the vibrating air-cooling beds is 50 Hz, and the vibration intensity is 0-30000.