Production process of glass fiber accessory

Through hot pressing treatment and curing technology, the problem of poor adhesion and fixation effect of glass fiber accessories is solved, which improves the degree of bonding and yield and reduces costs.

CN118927691APending Publication Date: 2024-11-12SHENZHEN CDL PRECISION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411200870.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

As the base material for electronic equipment accessories, glass fiber has problems such as poor adhesion and fixation effect and high cost, resulting in a low yield.

Method used

The glass fiber substrate and the composite film are heat-pressed by a hot pressing mold to melt the glass fiber substrate and fuse it with the composite film, and then cool and cure the mercury lamp to improve the degree of bonding.

Benefits of technology

It effectively improves the adhesion of glass fiber accessories, avoids loosening of film and substrate, improves yield, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118927691A_ABST
    Figure CN118927691A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electronic equipment accessories, in particular to a production process of a glass fiber accessory, which comprises the following steps: A, respectively manufacturing a glass fiber base material and a composite film; b, transferring the glass fiber base material and the composite film into a hot pressing mold for stacking; c, performing hot-pressing treatment on the glass fiber base material and the composite film through a hot-pressing mold, so that the glass fiber base material is melted, and the composite film and the glass fiber base material are fused with each other; and D, carrying out curing treatment on the glass fiber base material and the composite film to form the glass fiber accessory. The glass fiber base material and the composite film are subjected to hot pressing treatment, so that the glass fiber base material is melted in the hot pressing process so as to be reliably attached to the composite film, that is, after the glass fiber base material is cooled and cured, a part of layered structure of the composite film can be integrated with the glass fiber base material, and therefore the bonding degree of the glass fiber base material and the composite film is improved; therefore, the phenomenon that the film and the base material of the electronic equipment accessory prepared by the method are not loosened is avoided, and the yield is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electronic equipment accessories, and in particular to a production process of glass fiber accessories. Background Art

[0002] At present, glass fiber is used as the base material for electronic equipment accessories, such as mobile phone cases and tablet back covers. However, due to the characteristics of glass fiber itself, the adhesion and fixation effect between glass fiber and the corresponding structure of the composite film (such as the ink layer, etc.) is not good, and although glass fiber has good performance, it is expensive, resulting in high cost and low yield when glass fiber is used as the base material for electronic equipment accessories. Summary of the invention

[0003] In view of the problems of the prior art, the present invention provides a production process for glass fiber accessories, which can improve the bonding effect between the glass fiber substrate and the composite film to improve the yield.

[0004] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0005] The present invention provides a production process for glass fiber accessories, comprising the following steps:

[0006] A. Prepare glass fiber substrate and composite membrane separately;

[0007] B. Transfer the glass fiber substrate and the composite film to a hot pressing mold for stacking;

[0008] C. hot pressing the glass fiber substrate and the composite film through a hot pressing mold to melt the glass fiber substrate so that the composite film and the glass fiber substrate are fused with each other;

[0009] D. Curing the glass fiber substrate and the composite film to form glass fiber accessories.

[0010] Further, step D specifically includes:

[0011] D1. Cooling and solidifying the glass fiber substrate and the composite film after hot pressing;

[0012] D2. Remove the protective layer from the composite film after cooling and solidification;

[0013] D3. The glass fiber substrate and the composite film treated in step D2 are cured by a mercury lamp;

[0014] Wherein, the energy of the mercury lamp in step D3 is 600-1500mj.

[0015] Furthermore, in step C, the temperature of the hot pressing molding is 120-170° C., and the duration of the hot pressing treatment is 1-5 min.

[0016] Further, in step A, the preparation of the composite film specifically includes:

[0017] A1. Print the outer texture layer on the protective layer;

[0018] A2. Printing medium varnish on one end of the outer texture layer away from the protective layer to form a varnish layer;

[0019] A3. Electroplating is performed at one end of the varnish layer away from the outer texture layer to form a segment coating;

[0020] A4. Print the inner texture layer at the end of the electroplating layer away from the varnish layer;

[0021] A5. Printing pattern structure at one end of the inner texture layer away from the segment coating;

[0022] Wherein, in step B, the pattern structure is bonded to the glass fiber substrate.

[0023] Furthermore, step A5 specifically includes:

[0024] A51. Print the LOGO layer on the end of the electroplating layer away from the varnish layer;

[0025] A52. Obtain the number n of ink layers to be printed; wherein n is a natural number greater than 0;

[0026] A53. Print an ink layer at one end of the LOGO layer away from the electroplating layer, and then perform a baking treatment;

[0027] A54. Execute step A53 (n-1) times.

[0028] Furthermore, in step A53, the thickness of the ink layer is 5-8 μm, the temperature of the baking treatment is 60-90° C., and the time of the baking treatment is 10-80 min.

[0029] Furthermore, a protective layer is provided for performing step A1, and the protective layer is provided with a release layer;

[0030] In step A1, the outer texture layer is transferred onto the release layer.

[0031] Furthermore, between steps A1 and A2, A4 and A5, the steps further include:

[0032] The outer texture layer / inner texture layer is illuminated by LED light;

[0033] Irradiation is performed through a mercury lamp and an outer texture layer / inner texture layer;

[0034] Among them, the energy of LED lamps is 400-1000mj, and the energy of mercury lamps is 600-1500mj.

[0035] Furthermore, it also includes:

[0036] E. CNC cutting of fiberglass accessories;

[0037] F. Check the size and appearance of the fiberglass parts after CNC cutting;

[0038] G. Obtain inspection results and process fiberglass accessories based on the inspection results.

[0039] Beneficial effects of the present invention: The present invention performs a hot pressing treatment on the glass fiber substrate and the composite film so that the glass fiber substrate melts during the hot pressing process, thereby being reliably bonded to the composite film, that is, after the glass fiber substrate is cooled and solidified, part of the layered structure of the composite film will be integrated with the glass fiber substrate, thereby improving the bonding degree between the two, so as to ensure that the electronic equipment accessories prepared by the present invention will not have the phenomenon of the film and the substrate loosening, and the yield is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 It is a process diagram of the present invention.

[0041] Figure 2 A schematic diagram of an embodiment of an electronic device accessory made according to the present invention.

[0042] Figure numerals: 1—protective layer, 2—external texture layer, 3—varnish layer, 4—electroplating layer, 5—inner texture layer, 6—pattern structure, 7—LOGO layer, 8—ink layer, 9—release layer, 10—glass fiber substrate. DETAILED DESCRIPTION

[0043] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with the embodiments and drawings, and the contents mentioned in the embodiments are not intended to limit the present invention. The present invention is described in detail below in conjunction with the drawings.

[0044] like Figure 1 and Figure 2 As shown, the present invention provides a production process for glass fiber accessories, comprising the following steps:

[0045] A. preparing a glass fiber substrate 10 and a composite membrane respectively;

[0046] B. transferring the glass fiber substrate 10 and the composite film to a hot pressing mold for stacking;

[0047] C. hot pressing the glass fiber substrate 10 and the composite film through a hot pressing mold, so that the glass fiber substrate 10 melts and the composite film and the glass fiber substrate 10 fuse with each other;

[0048] D. Curing the glass fiber substrate 10 and the composite film to form a glass fiber accessory.

[0049] In actual use, the glass fiber substrate 10 is pre-impregnated glass fiber or thermoplastic glass fiber, and the specific thickness and specifications can be prepared according to actual needs. The glass fiber substrate 10 has undergone a cooling and solidification molding during molding. The core of the present invention is: the glass fiber substrate 10 and the composite film are aligned and then hot pressed, and the glass fiber substrate 10 is melted by the high temperature of hot pressing, so that the composite film partially "penetrates" into the glass fiber substrate 10; the subsequent curing treatment makes the glass fiber substrate 10 solid again, and at this time the composite film is bonded to the glass fiber substrate 10 and will not fall off, thereby improving the yield.

[0050] Compared with the currently commonly used methods such as gluing between the glass fiber substrate 10 and the composite film, the glass fiber accessories produced by the present invention can ensure that the glass fiber substrate 10 and the composite film are not separated, thereby improving the yield of the glass fiber accessories and effectively reducing the production cost of the glass fiber accessories.

[0051] In this embodiment, step D specifically includes:

[0052] D1. Cooling and curing the glass fiber substrate 10 and the composite film after the hot pressing treatment; specifically, cooling and curing is to reduce the temperature of the glass fiber accessories to room temperature;

[0053] D2. Remove the protective layer 1 from the composite film after cooling and curing;

[0054] D3. The glass fiber substrate 10 and the composite film treated in step D2 are cured by a mercury lamp;

[0055] Wherein, the energy of the mercury lamp in step D3 is 600-1500mj.

[0056] That is, the curing process of the present invention is divided into two steps: the first step is to cure the glass fiber substrate 10 for the second time by cooling, so that the composite film and the glass fiber substrate 10 are tightly bonded and inseparable; then the protective layer 1 of the composite film needs to be torn off, and then the mercury lamp irradiation curing is carried out, which can effectively increase the hardness and adhesion of the surface of the glass fiber accessories, so that the strength of the glass fiber accessories meets the requirements and can attach the required components.

[0057] Specifically, in step C, the temperature of the hot pressing molding is 120-170° C., and the duration of the hot pressing treatment is 1-5 minutes.

[0058] Since the melting point of the prepreg glass fiber and the thermoplastic glass fiber is not high, it is only necessary to maintain a specific temperature for a short time to ensure reliable bonding between the glass fiber substrate 10 and the composite film. In the subsequent cooling and curing, it is equivalent to the glass fiber substrate 10 undergoing secondary cooling and curing, which can significantly change the performance of the glass fiber substrate 10. The secondary curing combined with mercury lamp irradiation allows the overall strength and adhesion of the glass fiber accessories to meet the requirements.

[0059] Specifically, in step A, the preparation of the composite film specifically includes:

[0060] A1. Transfer printing outer texture layer 2 on protective layer 1;

[0061] A2. Printing medium varnish on one end of the outer texture layer 2 away from the protective layer 1 to form a varnish layer 3;

[0062] A3. Electroplating is performed at one end of the varnish layer 3 away from the outer texture layer 2 to form a segment coating;

[0063] A4. Transfer printing the inner texture layer 5 at one end of the electroplating layer 4 away from the varnish layer 3;

[0064] A5. Printing pattern structure 6 at one end of the inner texture layer 5 away from the segment coating;

[0065] In step B, the pattern structure 6 is bonded to the glass fiber substrate 10 .

[0066] In actual operation, step A5 specifically includes:

[0067] A51. Printing LOGO layer 7 at one end of the electroplating layer 4 away from the varnish layer 3;

[0068] A52. Obtain the number n of ink layers 8 to be printed; wherein n is a natural number greater than 0;

[0069] A53. The ink layer 8 is printed on one end of the LOGO layer 7 away from the electroplating layer 4, and then baked;

[0070] A54. Execute step A53 (n-1) times.

[0071] That is, the ink layer 8 is used to reliably bond with the glass fiber substrate 10, and the other layered structures are located outside the glass fiber substrate 10, and cooperate with each other to achieve the desired visual / performance effects.

[0072] The following is an overview of the structure of the composite membrane:

[0073] The composite film prepared by the present invention comprises a protective layer 1, an outer texture layer 2, a varnish layer 3, an electroplating layer 4, an inner texture layer 5 and a pattern structure 6, wherein the electroplating layer 4 is arranged at one end of the inner texture layer 5 away from the pattern structure 6, the varnish layer 3 is arranged at one end of the electroplating layer 4 away from the inner texture layer 5, the varnish layer 3 is used to increase the adhesion between the outer texture layer 2 and the electroplating layer 4, and the outer texture layer 2 is arranged between the varnish layer 3 and the protective layer 1;

[0074] The pattern structure 6 is used to connect to an external substrate and is fixed to the substrate by heat pressing.

[0075] Specifically, the pattern structure 6 of the present invention is used to bond with an external substrate, and the substrate is preferably glass fiber. The two bonded layers are then hot-pressed and fixed. At a high temperature, the glass fiber will melt, which is equivalent to allowing the pattern structure 6 to be integrated into the substrate. The two are then cooled and solidified to ensure reliable bonding between the pattern structure 6 and the substrate, and to effectively ensure that the substrate and the pattern structure 6 will not separate. The pattern structure 6 is reliably connected to the protective layer 1, the outer texture layer 2, the varnish layer 3, the electroplating layer 4, and the inner texture layer 5 in sequence, and will not separate.

[0076] Therefore, through this embodiment, the yield rate of electronic equipment accessories can be effectively improved, achieving the purpose of reducing costs.

[0077] In this embodiment, the varnish layer 3 is disposed on the outer texture layer 2 by screen printing, and the thickness of the varnish layer 3 is 2-5 μm. The varnish layer 3 plays a connecting role, and as a bonding medium, it has a large adhesion with the outer texture layer 2 and the electroplating layer 4, thereby effectively ensuring that the outer texture layer 2 will not be deformed. Specifically, the varnish layer 3 is attached to the outer texture layer 2 at a temperature of 80-90°C and a time of 60-80 minutes.

[0078] In this embodiment, the electroplating layer 4 is made by optical electroplating or magnetron electroplating, and the thickness of the electroplating layer 4 is 30-300nm. The thickness of the electroplating layer 4 is determined by the effect on color and luster, rather than the thickness of the electronic device accessories. That is, the electroplating layer 4 is mainly set to adjust the overall visual effect of the present invention.

[0079] In this embodiment, the pattern structure 6 includes a LOGO layer 7 and an ink layer 8 , and the LOGO layer 7 is disposed between the ink layer 8 and one end of the inner texture layer 5 away from the electroplating layer 4 .

[0080] Specifically, the LOGO layer 7 and the ink layer 8 are printed successively, and the ink layer 8 is in contact with the external glass fiber substrate 10, so that the ink layer 8 and the glass fiber substrate 10 are reliably bonded during hot pressing; in addition, the ink layer 8 is also used to cooperate with the inner texture layer 5, so that the present invention can present the desired and more complex color effects; and the thickness of the ink layer 8 of this embodiment is 5-8μm.

[0081] Of course, the specific number of ink layers 8 can be set according to actual needs. The thickness of each ink layer 8 must be 5-8 μm to ensure that the ink layer 8 is stable.

[0082] In this embodiment, the protective layer 1 is provided with a release layer 9, and the release layer 9 is connected to the outer texture layer 2. That is, after the present embodiment is bonded to the glass fiber substrate 10 by hot pressing and cooling and solidification, the protective layer 1 can be separated from the present embodiment by tearing off the protective layer 1, and the release layer 9 ensures that the outer texture layer 2 will not be separated from the protective layer 1 and carried away or deformed.

[0083] In this embodiment, the outer texture layer 2 is disposed on the protective layer 1 by a pad printing process, and the thickness of the outer texture layer 2 is 6-12 μm.

[0084] In this embodiment, the inner texture layer 5 is disposed on the electroplating layer 4 by a pad printing process, and the thickness of the inner texture layer 5 is 6-12 μm.

[0085] The outer texture layer 2 and the inner texture layer 5 are both made of glue, and are directly attached to the protective layer 1 / electroplating layer 4 according to the required pattern and shape, and then solidified by irradiation with LED lamps and mercury lamps in succession, so as not to deform; during the hot pressing process, the inner texture layer 5 and the outer texture layer 2 which have been formed themselves will not melt again.

[0086] Specifically, in step A53, the thickness of the ink layer 8 is 5-8 μm, the baking temperature is 60-90° C., and the baking time is 10-80 min.

[0087] In this embodiment, steps A1 and A2, A4 and A5 also include:

[0088] The outer texture layer 2 / inner texture layer 5 is illuminated by LED lights;

[0089] Irradiation is performed through a mercury lamp and the outer texture layer 2 / inner texture layer 5;

[0090] Among them, the energy of LED lamps is 400-1000mj, and the energy of mercury lamps is 600-1500mj.

[0091] The optimum thickness of the inner texture layer 5 and the outer texture layer 2 is 6-12 μm.

[0092] In this embodiment, the thickness of the protective layer 1 (excluding the release layer 9) is optimally 0.075-0.125, which can ensure strength and be easy to tear off.

[0093] In this embodiment, the present invention further includes:

[0094] E. CNC cutting of fiberglass accessories;

[0095] F. Check the size and appearance of the fiberglass parts after CNC cutting;

[0096] G. Obtain inspection results and process fiberglass accessories based on the inspection results.

[0097] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention is disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with the profession can make some changes or modifications to equivalent embodiments of equivalent changes by using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent changes and modifications made to the above embodiments according to the technology of the present invention are within the scope of the technical solution of the present invention without departing from the content of the technical solution of the present invention.

Claims

1. A production process for glass fiber accessories, characterized in that: The following steps are involved: A. Prepare glass fiber substrate and composite membrane separately; B. Transfer the glass fiber substrate and the composite film to a hot pressing mold for stacking; C. hot pressing the glass fiber substrate and the composite film through a hot pressing mold to melt the glass fiber substrate so that the composite film and the glass fiber substrate are fused with each other; D. Curing the glass fiber substrate and the composite film to form glass fiber accessories.

2. The production process of glass fiber accessories according to claim 1, characterized in that: Step D specifically includes: D1. Cooling and solidifying the glass fiber substrate and the composite film after hot pressing; D2. Remove the protective layer from the composite film after cooling and solidification; D3. The glass fiber substrate and the composite film treated in step D2 are cured by a mercury lamp; Wherein, the energy of the mercury lamp in step D3 is 600-1500mj.

3. The production process of glass fiber accessories according to claim 1, characterized in that: In step C, the temperature of the hot pressing molding is 120-170° C., and the duration of the hot pressing treatment is 1-5 minutes.

4. The production process of glass fiber accessories according to claim 1, characterized in that: In step A, the preparation of the composite membrane specifically includes: A1. Transfer print the outer texture layer on the protective layer; A2. Printing medium varnish on one end of the outer texture layer away from the protective layer to form a varnish layer; A3. Electroplating is performed at one end of the varnish layer away from the outer texture layer to form a segment coating; A4. Print the inner texture layer at the end of the electroplating layer away from the varnish layer; A5. Printing pattern structure at one end of the inner texture layer away from the segment coating; Wherein, in step B, the pattern structure is bonded to the glass fiber substrate.

5. The production process of glass fiber accessories according to claim 4, characterized in that: Step A5 specifically includes: A51. Print the LOGO layer on the end of the electroplating layer away from the varnish layer; A52. Obtain the number n of ink layers to be printed; wherein n is a natural number greater than 0; A53. Print an ink layer at one end of the LOGO layer away from the electroplating layer, and then perform a baking treatment; A54. Execute step A53 (n-1) times.

6. The production process of glass fiber accessories according to claim 5, characterized in that: In step A53, the thickness of the ink layer is 5-8 μm, the temperature of the baking treatment is 60-90° C., and the time of the baking treatment is 10-80 min.

7. The production process of glass fiber accessories according to claim 4, characterized in that: Providing a protective layer for performing step A1, wherein the protective layer is provided with a release layer; In step A1, the outer texture layer is transferred onto the release layer.

8. The production process of glass fiber accessories according to claim 4, characterized in that: The steps A1 and A2, A4 and A5 also include: The outer texture layer / inner texture layer is illuminated by LED light; Irradiation is performed through a mercury lamp and an outer texture layer / inner texture layer; Among them, the energy of LED lamps is 400-1000mj, and the energy of mercury lamps is 600-1500mj.

9. The production process of glass fiber accessories according to claim 1, characterized in that: Also includes: E. CNC cutting of fiberglass accessories; F. Check the size and appearance of the fiberglass parts after CNC cutting; G. Obtain inspection results and process fiberglass accessories based on the inspection results.