A kind of water-based adhesive based on polyurethane and its manufacturing method
By preparing the polytetrahydrofuran ether glycol modified with bridge ring structure and branched hydrophilic chain extender, and modifying the aqueous polyurethane adhesive, the heat resistance and water resistance problems in high temperature and high humidity environment are solved, and the problem of heat resistance and water resistance in high temperature and high humidity environment is achieved. Higher mechanical strength and bonding properties.
Patent Information
- Application Number
- CN202410819500.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-06-24
AI Technical Summary
Water-based polyurethane adhesives have poor heat resistance and water resistance in high temperature and high humidity environments, resulting in a decrease in bonding strength and need to be modified to maintain good bonding properties.
By preparing polytetrahydrofuran ether glycol modified with bridge ring structure at the end of the molecular chain and a sulfide-type branched hydrophilic chain extender with branched structure, an aqueous polyurethane dispersion is formed, and the polyurethane is improved by specific manufacturing methods The stability and density of the molecular chain enhance the mechanical strength and density of the film.
It significantly improves the high temperature resistance and hydrolysis resistance of polyurethane adhesives, enhances the bonding performance, and maintains a good service life in high temperature and high humidity environments.
Smart Images

Figure CN118546645B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to a polyurethane-based water-based adhesive and a preparation method thereof. Background Art
[0002] In recent years, the use of adhesives has been increasing in all walks of life. Currently, the more common adhesives mainly include acrylic adhesives, epoxy resin adhesives and polyurethane adhesives. Among them, polyurethane adhesives have a large number of polar groups. These groups can chemically bond with the surfaces of various materials to ensure the firmness and durability of the joints. Therefore, they can show excellent bonding properties to various materials such as metals, plastics, rubber, and wood.
[0003] According to different usage systems, polyurethane adhesives can be mainly divided into three types: solvent-based, solvent-free and water-based polyurethane adhesives. Compared with traditional solvent-based polyurethane adhesives, polyurethane water-based adhesives use water as solvent and have extremely low volatile organic compounds (VOCs) content, which greatly reduces pollution to the environment. In addition, water-based adhesives are non-toxic and odorless, harmless to the human body, and are conducive to improving the working environment. Therefore, they are more in line with environmental protection requirements under the current context.
[0004] However, the heat resistance and water resistance of water-based polyurethane adhesives are poor, and the heat resistance is poor in high temperature and high humidity environments: in high temperature and high humidity environments, the urethane bonds (—NHCOO—) in polyurethane water-based adhesives are easily hydrolyzed, resulting in reduced bonding strength. Therefore, the water-based polyurethane adhesive needs to be modified so that it can have good bonding properties in extreme environments such as high temperature and high humidity.
[0005] Based on this, the present invention provides a water-based polyurethane adhesive, which not only has good bonding properties but also can maintain its service life in extreme environments of high temperature and high humidity. Summary of the invention
[0006] In order to solve the problems mentioned in the background technology, the object of the present invention is to provide a polyurethane-based water-based adhesive and a method for preparing the same.
[0007] The purpose of the present invention can be achieved through the following technical solutions:
[0008] A method for preparing a polyurethane-based water-based adhesive, wherein the water-based adhesive comprises the following components in parts by mass:
[0009] 75-85 parts of polyurethane aqueous dispersion;
[0010] Defoaming agent 0.1-0.3 parts;
[0011] Thickener 0.2-0.5 parts;
[0012] 4-8 parts of curing agent;
[0013] 30-50 parts of purified water;
[0014] The preparation method of the polyurethane aqueous dispersion comprises the following steps:
[0015] Step T1, placing the polytetramethylene glycol modified body under a temperature condition of 100-120° C. for vacuum dehydration for 1-2 hours, lowering the temperature to 40-50° C., then adding acetone, mechanically stirring evenly, then adding the diisocyanate monomer and the metal tin catalyst to the system, after the addition, keeping the temperature for 1-2 hours, then adding the branched hydrophilic chain extender, and raising the temperature to 70-80° C., keeping the temperature for reaction for 2-4 hours, to form a polyurethane pre-reacted body;
[0016] Step T2, lowering the temperature to 40-50° C., adding acetone to the polyurethane pre-reactant to reduce viscosity, and then adding a sulfonic acid hydrophilic chain extender, reacting for 20-40 minutes to form a polyurethane aqueous dispersion;
[0017] The manufacturing method comprises the following steps:
[0018] Step T10, mixing the polyurethane aqueous dispersion with purified water, emulsifying at high speed shear for 30-60 minutes, and then distilling under reduced pressure to remove acetone to form a polyurethane emulsion;
[0019] Step T20, add defoamer to the polyurethane emulsion, stir mechanically for 10-20 minutes after addition, let stand to defoam, then add thickener, continue stirring for 10-20 minutes, and finally add curing agent, stir and mix well.
[0020] As a further embodiment of the present invention, the defoamer is any one of BYK-019, BYK-024 or BYK-1730; the thickener is a non-ionic polyurethane thickener; and the curing agent is a water-based polyisocyanate curing agent.
[0021] As a further embodiment of the present invention, in step T1, the preparation method of the polytetrahydrofuran ether diol modified body is as follows:
[0022] Polytetrahydrofuran ether diol, 2,3-epoxypropylnorbornane and tetrahydrofuran are added to the reactor in sequence. After the addition is completed, nitrogen is introduced to exhaust the air, stirring is started, and after a uniform mixed liquid is formed, the temperature of the reaction liquid is gradually increased to 60-70° C., and then a phase transfer catalyst is added to the reactor. After the addition is completed, the reaction is continued for 2-4 hours under stirring conditions, and then the reaction is stopped, the nitrogen is removed, reduced pressure distillation is carried out, and the material is discharged by cooling to obtain a polytetrahydrofuran ether diol modified body.
[0023] As a further embodiment of the present invention, the number average molecular weight of the polytetramethylene ether diol is 2000.
[0024] As a further embodiment of the present invention, the molar ratio of the polytetramethylene ether glycol to the 2,3-epoxypropylnorbornane is 1:2.
[0025] As a further embodiment of the present invention, the phase transfer catalyst is boron trifluoride ether complex.
[0026] Specifically, boron trifluoride etherate is used as a phase transfer catalyst to catalyze the ring-opening addition of the active substituted hydroxyl group at the end of the polytetramethylene ether diol structure and the epoxy group in the 2,3-epoxypropylnorbornane structure. By controlling the dosage ratio of the two, a polytetramethylene ether diol modified body containing two equivalent bridge ring structures at the end of the structure is obtained. Since new hydroxyl groups are generated during the ring-opening reaction, it can be used as a soft segment monomer of polyurethane and participate in the subsequent polymerization process of polyurethane.
[0027] As a further embodiment of the present invention, in step T1, the preparation method of the branched hydrophilic chain extender is as follows:
[0028] Add trimethylolpropane tris(thioglycolic acid) and toluene solvent to a reactor filled with nitrogen in sequence. After the addition is completed, start stirring. After a uniform mixed solution is formed, add 3-bromo-2-bromomethylpropionic acid to the reactor. After shaking, raise the temperature of the reaction solution to 70-80°C. After stirring for 2-3 hours, add an alkaline promoter to the reactor, continue the reaction for 6-9 hours, remove the nitrogen, remove the solvent by reduced pressure distillation, cool and discharge, and the branched hydrophilic chain extender can be obtained.
[0029] As a further embodiment of the present invention, the molar ratio of trimethylolpropane tris(thioglycolic acid) to 3-bromo-2-bromomethylpropionic acid is 1:1-1.5.
[0030] As a further embodiment of the present invention, the alkaline promoter is triethylamine or pyridine.
[0031] Specifically, the highly active thiol substituent in the structure of trimethylolpropane tris(thioglycolic acid) and the halogen substituent in the structure of 3-bromo-2-bromomethylpropionic acid can undergo a continuous substitution reaction under the action of an alkaline promoter. By controlling the amount of the reactants, they can be continuously polymerized to form a product having a thioether-type branched structure and containing a large number of substituted carboxyl groups, namely a branched hydrophilic chain extender.
[0032] As a further embodiment of the present invention, in step T2, the sulfonic acid hydrophilic chain extender is N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid.
[0033] A polyurethane-based water-based adhesive is prepared by adopting the above-mentioned manufacturing method.
[0034] Beneficial effects of the present invention:
[0035] (1) The present invention first prepares a polytetramethylene glycol modified product containing a bridge ring structure at the end of the molecular chain as a soft segment monomer, so that the prepared polyurethane aqueous dispersion structure contains a large number of rigid bridge ring structures. The presence of such rigid heterocycles can improve the stability of the polyurethane molecular chain and hinder the movement of the polyurethane molecular chain, thereby improving its shrinkage. Therefore, it can not only enhance the high temperature resistance of the waterborne polyurethane adhesive, but also make the adhesive film formed by curing the adhesive have higher mechanical strength.
[0036] (2) The present invention participates in the chain extension process of polyurethane by preparing a branched hydrophilic chain extender with a thioether-type branched structure. Since the branched hydrophilic chain extender structure contains multiple substituted mercapto groups, it can produce a branching effect during the polymerization of polyurethane, which is beneficial to improving the density of the polyurethane molecular chain. It can not only wrap the hydrolyzed groups in the polyurethane molecular chain to avoid direct contact with water, but also make the adhesive film have a higher density and produce a strong barrier effect on the penetration of water, thereby effectively improving the hydrolysis resistance of the water-based polyurethane adhesive. In addition, a large number of thioether structures can also produce a hydrogen bond effect with the adhered substrate, so it can also effectively enhance the bonding performance of the water-based polyurethane adhesive.
[0037] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for describing the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0039] Figure 1 This is the infrared analysis test diagram of the modified polytetramethylene ether diol;
[0040] Figure 2 This is the infrared analysis test diagram of the branched hydrophilic chain extender. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] The polyurethane aqueous dispersions used in the following examples were prepared by the following method:
[0043] Step T1, placing 20g of polytetrahydrofuran ether diol modified body at a temperature of 110°C for vacuum dehydration for 1h, lowering the temperature to 45°C, then adding 100mL of acetone, mechanically stirring evenly, then adding 8g of toluene-2,4-diisocyanate and 0.03g of dibutyltin dilaurate to the system, after the addition is completed, keeping the temperature for h, then adding 1g of branched hydrophilic chain extender, and raising the temperature to 75°C, keeping the temperature for reaction for 3h to form a polyurethane pre-reactor;
[0044] Step T2, lowering the temperature to 45° C., adding 50 mL of acetone to the polyurethane pre-reactant to reduce the viscosity, and then adding 0.05 g of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid, reacting for 30 minutes to form a polyurethane aqueous dispersion.
[0045] The preparation method of the polytetrahydrofuran ether diol modified body is as follows:
[0046] 5 g of polytetrahydrofuran ether diol with a number average molecular weight of 2000, 0.55 g of 2,3-epoxypropyl norbornane and tetrahydrofuran were added to the reactor in sequence. After the addition, nitrogen was introduced to exhaust the air, stirring was started until a uniform mixed liquid was formed, and the temperature of the reaction liquid was gradually increased to 65° C. Then 0.1 g of boron trifluoride ether complex was added to the reactor. After the addition was completed, the reaction was continued for 3 hours under stirring conditions, and the reaction was stopped. The nitrogen was removed, the vacuum distillation was carried out, and the material was discharged by cooling to obtain a polytetrahydrofuran ether diol modified body.
[0047] Figure 1 This is the infrared analysis test diagram of the modified polytetrahydrofuran diol, where 3290cm -1 The absorption peak at 2957 cm is the characteristic absorption peak of hydroxyl group. -1 and 2879cm -1 The characteristic absorption peaks of CH of methylene and methine appear at 1062cm -1 The absorption peak appearing at is the characteristic absorption peak of ether bond.
[0048] The preparation method of the branched hydrophilic chain extender is as follows:
[0049] Add 1.2 g of trimethylolpropane tris(thioglycolic acid) and toluene solvent to a reactor filled with nitrogen in sequence. After the addition, start stirring. After a uniform mixed solution is formed, add 1.2 g of 3-bromo-2-bromomethylpropionic acid to the reactor. After shaking, raise the temperature of the reaction solution to 75°C. After stirring for 3 hours, add 0.5 g of triethylamine to the reactor. Continue to react for 8 hours. Remove the nitrogen, remove the solvent by reduced pressure distillation, cool and discharge the material to obtain a branched hydrophilic chain extender.
[0050] Figure 2 This is the infrared analysis test diagram of the branched hydrophilic chain extender, where 2408cm -1 The absorption peak at 1757 cm is the characteristic absorption peak of thiol. -1 and 1704cm -1 The characteristic absorption peaks appearing at 1097 cm-1 are the C=O characteristic absorption peaks in the ester group and the C=O characteristic absorption peaks in the substituted carboxyl group. -1 The absorption peak appearing at is the characteristic absorption peak of SC.
[0051] Example 1
[0052] A polyurethane-based water-based adhesive comprising the following components in parts by mass:
[0053] 75 parts of polyurethane aqueous dispersion;
[0054] Defoamer BYK-019 0.1 part;
[0055] Thickener Vesmody U604 0.2 parts;
[0056] 4 parts of Desmodur DN isocyanate curing agent;
[0057] 30 parts of purified water;
[0058] The method for producing the water-based adhesive comprises the following steps:
[0059] Step T10, mixing the polyurethane aqueous dispersion with purified water, emulsifying at high speed shear for 30 minutes, and then distilling under reduced pressure to remove acetone to form a polyurethane emulsion;
[0060] Step T20, add defoamer BYK-019 to the polyurethane emulsion, stir mechanically for 10 minutes after addition, let stand to defoam, then add thickener, continue stirring for 10 minutes, and finally add Desmodur DN isocyanate curing agent, stir and mix well.
[0061] Example 2
[0062] A polyurethane-based water-based adhesive comprising the following components in parts by mass:
[0063] 80 parts of polyurethane aqueous dispersion;
[0064] Defoamer BYK-024 0.2 parts;
[0065] Thickener Vesmody U604 0.3 parts;
[0066] 5 parts of Desmodur DN isocyanate curing agent;
[0067] 40 parts of purified water;
[0068] The method for producing the water-based adhesive comprises the following steps:
[0069] Step T10, mixing the polyurethane aqueous dispersion with purified water, emulsifying at high speed shear for 40 minutes, and then distilling under reduced pressure to remove acetone to form a polyurethane emulsion;
[0070] Step T20, add defoamer BYK-024 to the polyurethane emulsion, stir mechanically for 15 minutes after addition, let stand to defoam, then add thickener, continue stirring for 15 minutes, and finally add Desmodur DN isocyanate curing agent, stir and mix well.
[0071] Example 3
[0072] A polyurethane-based water-based adhesive comprising the following components in parts by mass:
[0073] 85 parts of polyurethane aqueous dispersion;
[0074] Defoamer BYK-1730 0.3 parts;
[0075] Thickener Vesmody U604 0.5 part;
[0076] Desmodur DN isocyanate curing agent 8 parts;
[0077] 50 parts of purified water;
[0078] The method for producing the water-based adhesive comprises the following steps:
[0079] Step T10, mixing the polyurethane aqueous dispersion with purified water, emulsifying at high speed shear for 60 minutes, and then distilling under reduced pressure to remove acetone to form a polyurethane emulsion;
[0080] Step T20, add defoamer BYK-1730 to the polyurethane emulsion, stir mechanically for 20 minutes after addition, let stand to defoam, then add thickener, continue stirring for 20 minutes, and finally add Desmodur DN isocyanate curing agent, stir and mix well.
[0081] Comparative Example 1
[0082] A polyurethane-based water-based adhesive comprising the following components in parts by mass:
[0083] 80 parts of polyurethane aqueous dispersion;
[0084] Defoamer BYK-024 0.2 parts;
[0085] Thickener Vesmody U604 0.3 parts;
[0086] 5 parts of Desmodur DN isocyanate curing agent;
[0087] 40 parts of purified water;
[0088] The method for producing the water-based adhesive comprises the following steps:
[0089] Step T10, mixing the polyurethane aqueous dispersion with purified water, emulsifying at high speed shear for 40 minutes, and then distilling under reduced pressure to remove acetone to form a polyurethane emulsion;
[0090] Step T20, add defoamer BYK-024 to the polyurethane emulsion, stir mechanically for 15 minutes after addition, let stand to defoam, then add thickener, continue stirring for 15 minutes, and finally add Desmodur DN isocyanate curing agent, stir and mix well.
[0091] The method for preparing the aqueous polyurethane dispersion is different from that in the above embodiment in that the modified polytetramethylene ether diol is replaced by polytetramethylene ether diol, and the rest remains unchanged.
[0092] Comparative Example 2
[0093] A polyurethane-based water-based adhesive comprising the following components in parts by mass:
[0094] 80 parts of polyurethane aqueous dispersion;
[0095] Defoamer BYK-024 0.2 parts;
[0096] Thickener Vesmody U604 0.3 parts;
[0097] 5 parts of Desmodur DN isocyanate curing agent;
[0098] 40 parts of purified water;
[0099] The method for producing the water-based adhesive comprises the following steps:
[0100] Step T10, mixing the polyurethane aqueous dispersion with purified water, emulsifying at high speed shear for 40 minutes, and then distilling under reduced pressure to remove acetone to form a polyurethane emulsion;
[0101] Step T20, add defoamer BYK-024 to the polyurethane emulsion, stir mechanically for 15 minutes after addition, let stand to defoam, then add thickener, continue stirring for 15 minutes, and finally add Desmodur DN isocyanate curing agent, stir and mix well.
[0102] The method for preparing the aqueous polyurethane dispersion is different from that in the above embodiment in that the branched hydrophilic chain extender is replaced with conventional 2,2-dimethylolpropionic acid, and the rest remains unchanged.
[0103] Test Case
[0104] a. The adhesives in Examples 1 to 3 and Comparative Examples 1 to 2 were evenly coated on a clean PP substrate surface, and the adhesive was applied on one side. After 20 seconds, the substrate was bonded and then placed in a constant temperature box at 80°C for 8 hours to form a test sample. The peel strength test was performed according to the standard GB / T 2790-1995. Another test sample of the same specification was placed in an environment with a temperature of 85°C and a relative humidity of 85% for 10 days, then taken out, cooled naturally, and the peel strength was tested again to evaluate the high temperature and high humidity resistance of the adhesive.
[0105] b. Apply the adhesive evenly on the surface of a clean glass plate, place it in a constant temperature box at 80°C for 8 hours, then take it out and remove the film to form a film sample. According to the standard GB / T 1040.3-2006, test the tensile strength of the film; the test results are shown in the following table:
[0106] ,
[0107] Analysis of the test data shows that the adhesives prepared in Examples 1 to 3 of the present invention have significantly better bonding properties, strong high temperature and high humidity resistance, and can exhibit certain mechanical properties, while the polyurethane adhesive prepared using conventional polytetramethylene glycol as the soft segment has significantly worse mechanical properties, and its high temperature and high humidity resistance also decreases. The polyurethane adhesive prepared using conventional 2,2-dimethylol propionic acid chain extender has a relatively low degree of crosslinking, so its high temperature and high humidity resistance is extremely poor.
[0108] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A method for producing a polyurethane-based water-based adhesive, characterized in that: The water-based adhesive comprises the following components in parts by mass: 75-85 parts of polyurethane aqueous dispersion; Defoaming agent 0.1-0.3 parts; Thickener 0.2-0.5 parts; 4-8 parts of curing agent; 30-50 parts of purified water; The preparation method of the polyurethane aqueous dispersion comprises the following steps: Step T1, placing the polytetramethylene glycol modified body under a temperature condition of 100-120° C. for vacuum dehydration for 1-2 hours, lowering the temperature to 40-50° C., then adding acetone, mechanically stirring evenly, then adding the diisocyanate monomer and the metal tin catalyst to the system, after the addition, keeping the temperature for 1-2 hours, then adding the branched hydrophilic chain extender, and raising the temperature to 70-80° C., keeping the temperature for reaction for 2-4 hours, to form a polyurethane pre-reacted body; Step T2, lowering the temperature to 40-50° C., adding acetone to the polyurethane pre-reactant to reduce viscosity, and then adding a sulfonic acid hydrophilic chain extender, reacting for 20-40 minutes to form a polyurethane aqueous dispersion; The preparation method of the polytetrahydrofuran ether diol modified body is as follows: Add polytetrahydrofuran ether diol, 2,3-epoxypropylnorbornane and tetrahydrofuran to the reactor in sequence, introduce nitrogen after the addition, exhaust the air, start stirring, and gradually increase the temperature of the reaction liquid to 60-70° C. after forming a uniform mixed liquid, then add a phase transfer catalyst to the reactor, continue the reaction for 2-4 hours under stirring, stop the reaction, remove the nitrogen, perform reduced pressure distillation, cool and discharge the material, and obtain a polytetrahydrofuran ether diol modified body; The preparation method of the branched hydrophilic chain extender is as follows: Sequentially add trimethylolpropane tris(thioglycolic acid) and toluene solvent to a reactor filled with nitrogen, start stirring after adding, and after a uniform mixed solution is formed, add 3-bromo-2-bromomethylpropionic acid to the reactor, shake well, raise the temperature of the reaction solution to 70-80°C, stir for 2-3h, then add the alkaline promoter to the reactor, continue the reaction for 6-9h, remove the nitrogen, remove the solvent by vacuum distillation, cool and discharge, and obtain a branched hydrophilic chain extender; The manufacturing method comprises the following steps: Step T10, mixing the polyurethane aqueous dispersion with purified water, emulsifying at high speed shear for 30-60 minutes, and then distilling under reduced pressure to remove acetone to form a polyurethane emulsion; Step T20, add defoamer to the polyurethane emulsion, stir mechanically for 10-20 minutes after addition, let stand to defoam, then add thickener, continue stirring for 10-20 minutes, and finally add curing agent, stir and mix well.
2. The method for producing a polyurethane-based water-based adhesive according to claim 1, characterized in that: The number average molecular weight of the polytetramethylene ether diol is 2000.
3. The method for producing a polyurethane-based water-based adhesive according to claim 1, characterized in that: The molar ratio of the polytetramethylene ether glycol to the 2,3-epoxypropylnorbornane is 1:
2.
4. The method for producing a polyurethane-based water-based adhesive according to claim 1, characterized in that: The phase transfer catalyst is boron trifluoride ether complex.
5. The method for producing a polyurethane-based water-based adhesive according to claim 1, characterized in that: The molar ratio of the trimethylolpropane tris(thioglycolic acid) to 3-bromo-2-bromomethylpropionic acid is 1:1-1.
5.
6. The method for producing a polyurethane-based water-based adhesive according to claim 1, characterized in that: The alkaline promoter is triethylamine or pyridine.
7. The method for producing a polyurethane-based water-based adhesive according to claim 1, characterized in that: In step T2, the sulfonic acid hydrophilic chain extender is N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid.
8. A polyurethane-based water-based adhesive, characterized in that: The method according to claim 1 is used to prepare the present invention.
Citation Information
Patent Citations
Polyether containing bridge ring and preparation method thereof
CN106995365A
Castor oil-based hydrophilic chain extender as well as preparation method and application thereof
CN107556452A
Modified synthesis method of high-molecular waterborne polyurethane copper phthalocyanine coating
CN111100546A
Chain extender as well as preparation method and application thereof
CN112028801A
Waterborne polyurethane, and preparation method and application thereof
CN112159509A