An interface buffer multilayer gradient composite film and its preparation method and application
Through the design of the interface buffer multi-layer gradient composite film, the respiratory polymer buffer layer and gradient pore channel are used to solve the problem of separator damage and lithium dendrites during charging and discharging of lithium metal batteries, and improve the cycle life and safety of the battery performance.
Patent Information
- Application Number
- CN202410994360.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-07-24
AI Technical Summary
During the charging and discharging process of lithium metal batteries, the separator is damaged due to the change in the volume of lithium metal negative electrode, and the cycle life cannot be effectively improved. The existing technology is difficult to fundamentally solve the problem of lithium dendrites and lithium metal negative electrodes reacting with electrolyte, resulting in a decrease in battery capacity. and performance drops.
The multi-layer gradient composite membrane is adopted to provide gradient pore channels and respiratory polymer buffer layers through chemically grafted respiratory polymer buffer layers and multi-layer gradient composite membrane structures to alleviate the expansion and contraction of lithium metal electrodes. Promote the uniform deposition and conduction of lithium ions and inhibit the growth of lithium dendrites.
It effectively improves the cycle life and safety performance of lithium metal batteries, slows down the pressure and interface damage between the electrodes, promotes ion transmission, and extends the service life of the battery.
Smart Images

Figure CN118554130B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of liquid and semi-solid lithium metal batteries, and in particular to an interface buffer multilayer gradient composite film and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are widely used in mobile electronic devices such as mobile phones, laptops, and cameras. In recent years, with the development of electric vehicles and energy storage devices, the application areas of lithium-ion batteries have been greatly expanded, and higher requirements have been placed on their energy density and service life. In lithium-ion batteries, electrode materials account for about 30% to 40% of the total weight. In addition, the cycle stability of electrode materials is one of the important factors affecting the service life of lithium-ion batteries, so electrode materials are considered to be the key factors in determining battery energy density and service life.
[0003] At present, the specific capacity of carbon materials cannot meet people's requirements for energy density, while metallic lithium has the advantages of much higher specific capacity than carbon materials, lower electrode potential and smaller density. Therefore, metallic lithium is expected to become an ideal material to replace carbon materials as negative electrodes. However, lithium negative electrodes face many difficulties in practical applications, mainly due to the following reasons:
[0004] 1. Huge volume effect: The lithium metal negative electrode has no skeleton structure, so its relative volume change is infinitely expanded as the lithium metal is completely dissolved / deposited during the cycle, far exceeding the 10% volume effect of the graphite negative electrode. The huge volume effect causes the solid electrolyte interface layer (SEI) to be continuously broken and regenerated, resulting in serious loss of active substances;
[0005] 2. Poor safety performance: Uneven lithium deposition will form dendritic lithium dendrites on the surface of the metal lithium negative electrode, which may pierce the diaphragm after long-term circulation, causing battery short circuit, triggering or even explosion;
[0006] 3. Activity: The standard electrode potential of lithium metal is extremely low (3.04V vs. SHE). Almost no electrolyte can maintain the thermodynamic stability of lithium metal. Fresh lithium metal will react spontaneously when in contact with electrolyte. Lithium dendrites with high specific surface area intensify the side reaction. Dendrite breakage will form "dead lithium" that cannot contact the electrode.
[0007] 4. Severe electrode polarization: The volume expansion and high electrochemical activity of metallic lithium will inevitably lead to instability of the electrode / electrolyte interface (composition fluctuations and structural changes, fracture or even collapse of the solid electrolyte), resulting in continuous formation of new SEI in interface cracks, which will continue to accumulate with cycles, hindering the effective transmission of ions and causing severe electrode polarization. Therefore, when lithium metal is used as the negative electrode in solid-state batteries, there will be problems such as uneven lithium element deposition and dendrite generation during the charge and discharge process, which will lead to a decrease in battery capacity, performance drop or even failure.
[0008] In the prior art, stable lithium metal circulation is mainly achieved by constructing a stable SEI film on the surface of lithium metal. The improvement measures are mainly: by improving the components of the electrolyte, such as adding SEI film-forming additives to the electrolyte, so that lithium metal can generate a more stable SEI in situ during the electrochemical behavior. The defects of this method are: first, the mechanical modulus of the constructed SEI is small, which is not enough to inhibit the damage of lithium dendrites to SEI; second, the continuous consumption of electrolyte components such as additives will cause the performance of lithium metal to deteriorate in the later stage of the cycle; third, it takes a long time to form a stable SEI by immersion.
[0009] Therefore, solid-state batteries using lithium metal as the negative electrode will still have problems with uneven lithium deposition and dendrites during the charging and discharging process, which will lead to a decrease in battery capacity, performance degradation, or even failure. However, the technology is not yet mature for problems such as lithium dendrites and the reaction between the lithium metal negative electrode and the electrolyte, and a relatively mature solution has not yet been found. In addition, the expansion and contraction problem during the charging and discharging process of lithium metal batteries cannot be ignored, which directly affects the cycle life of lithium metal batteries. The prior art attempts to solve this technical problem with the help of external pressure, but the external pressure can only slow down the expansion, and it is difficult to fundamentally solve the technical problem, and excessive external pressure is also difficult to apply in practice. Summary of the invention
[0010] The present invention aims to overcome the problem that the lithium battery separator in the prior art cannot overcome the expansion and contraction problem of the existing lithium metal battery during the charging and discharging process. Therefore, an interface buffer multilayer gradient composite membrane and its preparation method and application are provided to overcome this technical problem.
[0011] In order to achieve the above invention objectives, the present invention is implemented through the following technical solutions:
[0012] In a first aspect, the present invention first provides an interface buffer multilayer gradient composite film,
[0013] It includes a multi-layer gradient composite membrane and a breathable polymer buffer layer chemically grafted on one side of the multi-layer gradient composite membrane;
[0014] The multilayer gradient composite membrane comprises pore channels for transporting lithium ions, and the pore diameters of the pore channels increase in sequence in a direction away from the breathing polymer buffer layer;
[0015] The quasi-breathing polymer buffer layer is composed of a comb polymer containing carbonyl groups.
[0016] As described in the background technology, the lithium metal battery in the prior art has a huge change in the relative volume of the lithium metal negative electrode during the charge and discharge process, and the diaphragm of the lithium metal battery used in the prior art is generally a polyolefin film with a porous structure. Therefore, the polyolefin film will gradually be damaged due to the expansion and contraction of the lithium metal negative electrode, resulting in the cycle life of the lithium metal battery cannot be effectively improved.
[0017] The most significant difference between the composite film in the present application and the polyolefin film in the prior art is that a breathing polymer buffer layer composed of a comb-like polymer is grafted on one side surface of the diaphragm by chemical grafting. Compared with the polymer with a cross-linked structure in the prior art, the comb-like polymer is composed of linear polymer chain segments, and there is no cross-linked structure between adjacent polymer chain segments. Therefore, the flexibility and elasticity of its molecular chain are relatively high, so that it can curl and fold under the action of external force, so that it has a certain degree of adjustability, so that it can adapt to the volume change of the lithium metal electrode during the charging and discharging process. During the charging and discharging process of the lithium battery, the polymer buffer layer can expand and contract with the positive and negative pole pieces, and can perform a breathing-like contraction and expansion buffer, thereby reducing the pressure between the pole pieces and interface damage.
[0018] At the same time, the comb polymer in the present application has a large number of carbonyl groups in its molecular structure. Since these carbonyl groups have good lithium affinity, they can also combine with lithium ions in the process of promoting the transmission of lithium ions, thereby forming a stable solid electrolyte interface (SEI) film on the surface of the lithium metal electrode. This film can prevent direct contact between lithium ions and electrolytes, reduce the occurrence of side reactions, and also alleviate the volume change of the lithium metal electrode during the charge and discharge process.
[0019] In addition, compared with the single-layer porous polyolefin film in the prior art, the film in the present application is a composite film with a multilayer structure. The characteristics of the multilayer structure give it pore channels with different pore size gradients, and the design of the multi-level pore structure enables the multilayer gradient composite membrane to not only screen and guide lithium ions at one level, but also optimize the flow of lithium ions at both the microscopic and macroscopic scales. This multi-scale optimization strategy can more effectively utilize the pore channels in the membrane, thereby achieving faster ion transfer and more uniform lithium deposition, inhibiting the growth of lithium dendrites, improving the safety performance of lithium metal batteries, and further improving the cycle life of the battery cell.
[0020] Therefore, in summary, the interfacial buffer multilayer gradient composite membrane in the present application protects the lithium metal negative electrode and promotes ion conduction and dredging by constructing a multilayer gradient composite membrane with a gradient pore structure and a breath-like polymer buffer layer, while the breath-like buffer layer alleviates the expansion and contraction problems of the lithium metal electrode during the charging and discharging process, which is reflected in the further improvement of the battery cycle life at the macroscopic battery level.
[0021] Preferably, the comb polymer further comprises pyrrole groups.
[0022] The inventors of the present application have found in experiments that pyrrole and polycarbonyl groups, as electron-rich functional groups, can effectively interact with lithium ions on the surface of lithium metal to promote the uniform deposition / stripping process of lithium ions. When pyrrole groups and carbonyl groups are present in the comb polymer at the same time, the affinity between lithium ions can be further improved, thereby further reducing the capacity loss of lithium metal batteries caused by lithium dendrite growth during the cycle process and improving the cycle life.
[0023] At the same time, the inventors of the present application also found that the presence of the pyrrole ring enables it to effectively intercept polysulfides through chemical adsorption or catalysis. This characteristic not only enhances the membrane's adsorption capacity for polysulfides, but also promotes the improvement of the cycle stability and efficiency of lithium metal batteries.
[0024] Preferably, the multilayer gradient composite membrane is obtained by sequentially composite a polyamide membrane, a porous polyethylene membrane and a porous cellulose membrane;
[0025] The quasi-breathing polymer buffer layer is chemically grafted onto the surface of the polyamide membrane.
[0026] The multilayer gradient composite membrane in the present application comprises a three-layer membrane structure, wherein the polyamide membrane contains amide groups, which have good affinity with lithium ions, thereby promoting the permeability of lithium ions. At the same time, it can also effectively intercept polysulfides through chemical adsorption or catalysis, thereby improving the adsorption capacity of the diaphragm for polysulfides, and also promoting the improvement of the cycle stability and efficiency of lithium metal batteries.
[0027] The setting of the porous polyethylene membrane can provide good support for the polyamide membrane, while the presence of the cellulose membrane can ensure the mechanical strength and support of the overall composite membrane while providing larger pores, preventing the diaphragm from being damaged during the volume change of the lithium metal electrode.
[0028] Preferably, the polyamide membrane contains nanometer-scale pores, and the porous polyethylene membrane contains micrometer-scale pores.
[0029] Preferably, the polyamide film further comprises anthraquinone groups.
[0030] The inventors of the present application have found in experiments that when anthraquinone groups are introduced into polyamide membranes, the number of carbonyl groups in the polyamide membranes can be effectively increased. At the same time, due to the chemical properties of the anthraquinone functional groups themselves, they can also interact with lithium salt ions intermolecularly. This interaction involves ion-dipole interaction to transport lithium ions, thereby improving the solubility of lithium salts and ion transmission efficiency.
[0031] In a second aspect, the present invention also provides a method for preparing the multilayer gradient composite membrane.
[0032] The method comprises the steps of placing a multilayer gradient composite membrane in a plasma atmosphere, introducing vapor of a reaction monomer containing a carbonyl group therein, thereby grafting a comb-shaped polymer on the surface of the multilayer gradient composite membrane to obtain a breathing polymer buffer layer.
[0033] The quasi-breathable polymer buffer layer in the present application is obtained by plasma enhanced chemical vapor deposition. Compared with the polymer obtained by polymerization in liquid form in the prior art, it can create grafting active points on the surface of the multilayer gradient composite membrane through plasma, so that the vapor of the reaction monomer containing the carbonyl group can continue to grow comb-shaped polymers along the active points, thereby obtaining a quasi-breathable polymer buffer layer. Therefore, the quasi-breathable polymer buffer layer in the present application is connected to the multilayer gradient composite membrane through a chemical bond, so the connection strength between the two is higher, so that its integrity can still be maintained under greater expansion and contraction.
[0034] The conventional method of obtaining the membrane layer by liquid phase polymerization usually relies on intermolecular forces to connect the multilayer gradient composite membrane, resulting in weak connection stability between the two. Under the expansion and contraction of the lithium metal negative electrode, peeling will occur, thus affecting the cycle life of the lithium metal battery.
[0035] Preferably, the reactive monomer is one or a combination of acrylic acid monomer, acrylamide monomer, methacrylic acid monomer, vinyl acetate, acrylyl pyrrole, and diacetone acrylamide monomer.
[0036] Preferably, the reaction monomer is a mixed gas of acrylyl pyrrole and diacetone acrylamide vapor; wherein,
[0037] The ratio of the acrylpyrrole to diacetone acrylamide vapor is 1:0.3-1:0.6.
[0038] Preferably, during the process of grafting the comb-like polymer, the vacuum degree is 100-1000 Pa, the reaction temperature is 60-80° C., and the reaction time is 12-48 h.
[0039] Preferably, the preparation method of the multilayer gradient composite membrane is as follows:
[0040] (S.1) hot-pressing a porous polyethylene stretched film and a porous cellulose film to obtain a double-layer composite film;
[0041] (S.2) dissolving a diamine monomer in an aqueous solvent to obtain an aqueous reaction solution;
[0042] dissolving the polyacyl chloride monomer in an oil phase organic solvent to obtain an oil phase reaction solution;
[0043] (S.3) The double-layer composite membrane is immersed in an aqueous reaction solution and then taken out, so that a layer of aqueous reaction solution adheres to the surface of the double-layer composite membrane. The double-layer composite membrane is then immersed in an oil-phase reaction solution, so that the diamine monomer on the surface of the double-layer composite membrane reacts with the polyacyl chloride monomer to form a polyamide membrane, thereby obtaining a multi-layer gradient composite membrane.
[0044] Preferably, the diamine monomer includes one or more of m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, xylylenediamine, ethylenediamine, propylenediamine, 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, piperazine, and 4-aminomethylpiperazine.
[0045] Preferably, the mass-volume concentration of the diamine monomer is 1-2 g / mL.
[0046] Preferably, the polyacyl chloride monomer includes one or more of isophthaloyl chloride, terephthaloyl chloride, 1,3,5-trimesoyl chloride, and 9,10-anthraquinone-2-sulfonyl chloride.
[0047] Preferably, the mass-volume concentration of the polyacyl chloride monomer is 0.5-1 g / mL
[0048] Preferably, the mass-volume concentration of the 9,10-anthraquinone-2-sulfonyl chloride monomer is 0.04-0.3 g / mL.
[0049] Preferably, the double-layer composite membrane is allowed to stand in the aqueous reaction solution for 10-60 min.
[0050] Preferably, the double-layer composite membrane is reacted in the oil phase reaction solution for 2-10 minutes.
[0051] Preferably, after the reaction is completed, the obtained multilayer composite film is heat-treated in a vacuum oven at 80-100° C. for 30-60 min.
[0052] In a third aspect, the present invention further provides a lithium metal battery, which comprises the interface buffer multilayer gradient composite film as described in any one of the above.
[0053] Therefore, the present invention has the following beneficial effects:
[0054] The present invention provides a method for preparing an interfacial buffer multilayer gradient composite membrane, and constructs a membrane with multiple layers of different pore structures for composite to form a gradient pore structure, wherein the outermost layer of the composite membrane is a quasi-breathing polymer buffer layer formed by grafting modification. The multilayer gradient composite membrane not only protects the lithium metal negative electrode, but also promotes ion conduction and dredging, while the quasi-breathing buffer layer alleviates the expansion and contraction problems of the lithium metal electrode during the charge and discharge process, which is reflected in the further improvement of the battery cycle life at the macroscopic battery level. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 Schematic diagram of the formation of a breathing buffer layer by surface grafting.
[0056] Figure 2 Schematic diagram of the formation of nanoporous polyamide layer by interfacial polymerization.
[0057] Figure 3 Schematic diagram of the composite of multilayer composite membrane and lithium metal.
[0058] Figure 4 Schematic diagram of the assembly of the battery cell structure of a lithium metal battery. DETAILED DESCRIPTION
[0059] The present invention is further described below in conjunction with specific embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should fall within the scope of protection of the present invention.
[0060] Embodiment 1:
[0061] Step 1: Prepare an interfacial polymerization reaction prepolymer solution. Dissolve a reaction monomer (piperazine) of the interfacial polymerization in a mixture of water and ethanol at room temperature, wherein the volume ratio of water to ethanol is 2:3, and stir for more than 2 hours to mix them evenly to obtain an interfacial polymerization aqueous phase reaction solution, wherein the mass-volume concentration of the piperazine monomer in the aqueous phase reaction solution is 1 g / mL;
[0062] Another monomer (1,3,5-benzene trimesoyl chloride) to be subjected to interfacial polymerization reaction was added to n-hexane at room temperature and stirred for 2 hours to mix evenly to obtain an interfacial polymerization oil phase reaction solution, wherein the mass-volume concentration of 1,3,5-benzene trimesoyl chloride monomer in the oil phase reaction solution was 0.5 g / mL.
[0063] Step 2: Press Figure 1The method shown is used to perform polymerization reaction to form a multilayer gradient composite membrane. The porous PE stretched film coated with glue on the surface is composited with a porous cellulose membrane by hot pressing to form a double-layer composite membrane (sample a). Sample a is immersed in the aqueous phase reaction solution prepared in step 1, and allowed to stand for 10 minutes. After being taken out and the surface reaction solution of sample a is scraped flat, it is immersed in the oil phase reaction solution prepared in step 1. After reacting for 10 minutes, the obtained multilayer composite membrane (sample b) is taken out and heat-treated in a vacuum oven at 80°C for 30 minutes to optimize the structure, fix the reaction product, obtain a multilayer gradient composite membrane, and store it in vacuum.
[0064] Step 3: If Figure 2 As shown, the membrane prepared in step 2 is placed under a plasma device, and the reaction monomer gas for constructing the buffer layer is introduced. A surface grafting reaction is carried out under a vacuum degree of 100 Pa, thereby creating grafting active points on the surface of the composite membrane and grafting a thin layer of molecules. Thereafter, the reaction gas is continuously introduced or the surface coating is carried out at 60°C for 12 hours to ensure sufficient polymerization reaction and obtain a surface grafted polymer layer sufficient to form a breathing effect.
[0065] The reactive monomers of the polymer buffer layer are a mixed gas of acryl pyrrole and diacetone acrylamide vapor;
[0066] The conditions of the plasma device are:
[0067] Select a plasma enhanced chemical vapor deposition device, the RF power source should be set at 13.56 MHz, and the power adjustment range should be 200 watts to control the energy output of the plasma and ensure that the diacetone acrylamide can react evenly and completely during the polymerization process;
[0068] The ratio of acrylpyrrole and diacetone acrylamide vapor is controlled at 1:0.3;
[0069] Gas flow rates: The flow rate of acryloyl pyrrole was set to 100 sccm (standard cubic centimeters per minute), and the flow rate of diacetone acrylamide vapor was 30 sccm.
[0070] Step 4: The interface buffer multilayer gradient composite film prepared in step 3 is cold pressed with the lithium metal negative electrode at a pressure of 1 MPa for 30 seconds to form a protective layer of the multi-interface buffer multilayer gradient composite film on the surface of the lithium metal negative electrode (its structure is as shown in FIG. Figure 3 The prepared modified negative electrode was stored in vacuum.
[0071] Step 5: Assemble the modified negative electrode (including the separator) prepared in step 4 with the positive electrode, the solid-liquid mixed electrolyte, the shell, etc. Figure 4 The semi-solid lithium metal battery cell structure is shown; the battery-related electrical and safety performance are tested, and the battery is comprehensively evaluated.
[0072] Example 2
[0073] Step 1: Prepare an interfacial polymerization reaction prepolymer solution. Dissolve a reaction monomer (m-phenylenediamine) of the interfacial polymerization in a mixture of water and ethanol at room temperature, wherein the volume ratio of water to ethanol is 2:3, and stir for more than 2 hours to mix them evenly to obtain an interfacial polymerization water phase reaction prepolymer, wherein the mass-volume concentration of the m-phenylenediamine monomer in the water phase reaction solution is 2 g / mL;
[0074] Another monomer (1,3,5-benzene trimesoyl chloride) to be subjected to interfacial polymerization reaction was added to n-hexane at room temperature and stirred for 4 hours to mix evenly to obtain an interfacial polymerization oil phase reaction solution, wherein the mass-volume concentration of 1,3,5-benzene trimesoyl chloride monomer in the oil phase reaction solution was 0.6 g / mL.
[0075] Step 2: Perform polymerization reaction to form a multilayer gradient composite membrane. The porous PE stretched film coated with glue on the surface is composited with the porous cellulose membrane by hot pressing to form a double-layer composite membrane (sample a). Sample a is immersed in the aqueous reaction solution prepared in step 1 and allowed to stand for 10 minutes. After being taken out and the surface reaction solution of sample a is scraped flat, it is immersed in the oil phase reaction solution prepared in step 1. After reacting for 10 minutes, the obtained multilayer composite membrane (sample b) is taken out and heat-treated in a vacuum oven at 100°C for 60 minutes, thereby optimizing the structure and fixing the reaction product to obtain a multilayer gradient composite membrane, which is then stored in a vacuum.
[0076] Step 3: Place the multilayer gradient composite membrane prepared in step 2 under a plasma device, introduce the reaction monomer gas for constructing the buffer layer, and carry out a surface grafting reaction under a vacuum degree of 1000 Pa; create grafting active points on the surface of the composite membrane and graft a thin layer of molecules, and then continue to introduce the reaction gas or carry out surface coating at 80°C for 24 hours to ensure sufficient polymerization reaction and obtain a surface grafted polymer layer sufficient to form a breathing effect.
[0077] The reactive monomers of the polymer buffer layer are a mixed gas of acryl pyrrole and diacetone acrylamide vapor;
[0078] The conditions of the plasma device are:
[0079] Select a plasma enhanced chemical vapor deposition device, the RF power source should be set at 13.56 MHz, and the power should be adjusted to 300 watts to control the energy output of the plasma and ensure that the diacetone acrylamide can react evenly and completely during the polymerization process;
[0080] The ratio of acrylpyrrole and diacetone acrylamide vapor is controlled at 1:0.4;
[0081] Gas flow rates: The flow rate of acryloyl pyrrole was set to 100 sccm (standard cubic centimeters per minute), and the flow rate of diacetone acrylamide vapor was 40 sccm.
[0082] Step 4: The interfacial buffer multilayer gradient composite film prepared in step 3 is cold pressed and composited with the lithium metal negative electrode at a pressure of 1 MPa for 30 seconds to form a protective layer of the multilayer gradient composite film on the surface of the lithium metal negative electrode, and the obtained modified negative electrode is stored in a vacuum.
[0083] Step 5: Assemble the modified negative electrode (including separator) prepared in step 4 with the positive electrode, solid-liquid mixed electrolyte, shell, etc. to form a semi-solid lithium metal battery; test the battery-related electrical properties and safety performance, and conduct a comprehensive evaluation of the battery.
[0084] Example 3
[0085] Step 1: Prepare an interfacial polymerization reaction prepolymer solution. Dissolve a reaction monomer (ethylenediamine) of the interfacial polymerization in a mixture of water and ethanol at room temperature, wherein the volume ratio of water to ethanol is 2:3, and stir for more than 2 hours to mix them evenly to obtain an interfacial polymerization aqueous phase reaction solution, wherein the mass-volume concentration of the ethylenediamine monomer in the aqueous phase reaction solution is 1.5 g / mL;
[0086] Another monomer (1,3,5-benzene trimesoyl chloride) to be subjected to interfacial polymerization reaction was added to n-hexane at room temperature and stirred for 7 hours to mix evenly to obtain an interfacial polymerization oil phase reaction solution, wherein the mass-volume concentration of 1,3,5-benzene trimesoyl chloride monomer in the oil phase reaction solution was 0.8 g / mL.
[0087] Step 2: Perform polymerization reaction to form a multilayer gradient composite membrane. The porous PE stretched film coated with glue on the surface is composited with the porous cellulose membrane by hot pressing to form a double-layer composite membrane (sample a). Sample a is immersed in the aqueous reaction solution prepared in step 1 and allowed to stand for 10 minutes. After being taken out and the surface reaction solution of sample a is scraped flat, it is immersed in the oil phase reaction solution prepared in step 1. After reacting for 10 minutes, the obtained multilayer composite membrane (sample b) is taken out and heat-treated in a vacuum oven at 90°C for 45 minutes to optimize the structure, fix the reaction product, obtain a multilayer gradient composite membrane, and store it in vacuum.
[0088] Step 3: Place the membrane prepared in step 2 under a plasma device, introduce the reaction monomer gas for constructing the buffer layer, and carry out a surface grafting reaction under a vacuum degree of 500 Pa, thereby creating grafting active points on the surface of the composite membrane and grafting a thin layer of molecules. Then, continue to introduce the reaction gas or carry out surface coating at 60°C for 48 hours to ensure sufficient polymerization reaction and obtain a surface grafted polymer layer sufficient to form a breathing effect.
[0089] The reactive monomers of the polymer buffer layer are a mixed gas of acryl pyrrole and diacetone acrylamide vapor;
[0090] The conditions of the plasma device are:
[0091] A plasma enhanced chemical vapor deposition device was selected, and the radio frequency power source was set at 13.56 MHz and the power was adjusted to 400 watts to control the energy output of the plasma and ensure that the diacetone acrylamide could react evenly and completely during the polymerization process;
[0092] The ratio of acrylpyrrole and diacetone acrylamide vapor is controlled at 1:0.5;
[0093] Gas flow rates: The flow rate of acryloyl pyrrole was set to 100 sccm (standard cubic centimeters per minute), and the flow rate of diacetone acrylamide vapor was set to 50 sccm (standard cubic centimeters per minute).
[0094] Step 4: The interfacial buffer multilayer gradient composite film prepared in step 3 is cold pressed and composited with the lithium metal negative electrode at a pressure of 1 MPa for 30 seconds to form a protective layer of the multilayer gradient composite film on the surface of the lithium metal negative electrode, and the obtained modified negative electrode is stored in a vacuum.
[0095] Step 5: Assemble the modified negative electrode (including separator) prepared in step 4 with the positive electrode, solid-liquid mixed electrolyte, shell, etc. to form a semi-solid lithium metal battery; test the battery-related electrical properties and safety performance, and conduct a comprehensive evaluation of the battery.
[0096] Example 4
[0097] Step 1: Prepare an interfacial polymerization reaction prepolymer solution. Dissolve a reaction monomer (piperazine) of interfacial polymerization in a mixture of water and ethanol at room temperature, wherein the volume ratio of water to ethanol is 2:3, and stir for more than 2 hours to mix them evenly to obtain an interfacial polymerization water phase reaction prepolymer, wherein the mass-volume concentration of the piperazine monomer in the water phase reaction solution is 1 g / mL;
[0098] Another monomer (1,3,5-benzene trimesoyl chloride) to be subjected to interfacial polymerization reaction was added to n-hexane at room temperature and stirred for 8 hours to mix evenly to obtain an interfacial polymerization oil phase reaction solution, wherein the mass-volume concentration of 1,3,5-benzene trimesoyl chloride monomer in the oil phase reaction solution was 0.9 g / mL.
[0099] Step 2: Perform polymerization reaction to form a multilayer gradient composite membrane. The porous PE stretched film coated with glue on the surface is composited with a porous cellulose membrane by hot pressing to form a double-layer composite membrane (sample a). Sample a is immersed in the aqueous reaction solution prepared in step 1 and allowed to stand for 10 minutes. After being taken out and the surface reaction solution of sample a is scraped flat, it is immersed in the oil phase reaction solution prepared in step 1. After reacting for 10 minutes, the obtained multilayer composite membrane (sample b) is taken out and heat-treated in a vacuum oven at 80°C for 30 minutes to optimize the structure, fix the reaction product, obtain a multilayer gradient composite membrane, and store it in vacuum.
[0100] Step 3: Place the membrane prepared in step 2 under a plasma device, introduce the reaction monomer gas for constructing the buffer layer, and carry out a surface grafting reaction under a vacuum degree of 100 Pa, thereby creating grafting active points on the surface of the composite membrane and grafting a thin layer of molecules. Then, continue to introduce the reaction gas at 70°C for 12 hours to ensure sufficient polymerization reaction and obtain a surface grafted polymer layer sufficient to form a breathing effect.
[0101] The reactive monomers of the polymer buffer layer are a mixed gas of acryl pyrrole and diacetone acrylamide vapor;
[0102] The conditions of the plasma device are:
[0103] Select a plasma enhanced chemical vapor deposition device, the RF power source should be set at 13.56 MHz, and the power should be adjusted to 400 watts to control the energy output of the plasma and ensure that the diacetone acrylamide can react evenly and completely during the polymerization process;
[0104] The ratio of acryl pyrrole and diacetone acrylamide vapor is controlled at 1:0.55;
[0105] Gas flow rates: The flow rate of acryloyl pyrrole was set to 100 sccm (standard cubic centimeters per minute), and the flow rate of diacetone acrylamide vapor was 55 sccm.
[0106] Step 4: The interfacial buffer multilayer gradient composite film prepared in step 3 is cold pressed and composited with the lithium metal negative electrode at a pressure of 0.5 MPa for 60 seconds to form a protective layer of the multilayer gradient composite film on the surface of the lithium metal negative electrode, and the obtained modified negative electrode is stored in a vacuum.
[0107] Step 5: Assemble the modified negative electrode (including separator) prepared in step 4 with the positive electrode, solid-liquid mixed electrolyte, shell, etc. to form a semi-solid lithium metal battery; test the battery-related electrical properties and safety performance, and conduct a comprehensive evaluation of the battery.
[0108] Example 5
[0109] Step 1: Prepare an interfacial polymerization reaction prepolymer solution. Dissolve a reaction monomer (piperazine) of interfacial polymerization in a mixture of water and ethanol at room temperature, wherein the volume ratio of water to ethanol is 2:3, and stir for more than 2 hours to mix them evenly to obtain an interfacial polymerization water phase reaction prepolymer, wherein the mass-volume concentration of the piperazine monomer in the water phase reaction solution is 1.2 g / mL;
[0110] Another monomer (1,3,5-benzene trimesoyl chloride) to be subjected to interfacial polymerization reaction was added to n-hexane at room temperature and stirred for 10 hours to mix evenly to obtain an interfacial polymerization oil phase reaction solution, wherein the mass-volume concentration of 1,3,5-benzene trimesoyl chloride monomer in the oil phase reaction solution was 1 g / mL.
[0111] Step 2: Perform polymerization reaction to form a multilayer gradient composite membrane. The porous PE stretched film coated with glue on the surface is composited with the porous cellulose membrane by hot pressing to form a double-layer composite membrane (sample a). Sample a is immersed in the aqueous reaction solution prepared in step 1 and allowed to stand for 10 minutes. After being taken out and the surface reaction solution of sample a is scraped flat, it is immersed in the oil phase reaction solution prepared in step 1. After reacting for 10 minutes, the obtained multilayer composite membrane (sample b) is taken out and heat-treated in a vacuum oven at 90°C for 30 minutes to optimize the structure, fix the reaction product, obtain a multilayer gradient composite membrane, and store it in vacuum.
[0112] Step 3: Place the membrane prepared in step 2 under a plasma device, introduce the reaction monomer gas for constructing the buffer layer, and carry out surface grafting reaction under a specific vacuum degree, generally 100Pa; create grafting active points on the surface of the composite membrane and graft a thin layer of molecules, and then continue to introduce the reaction gas or carry out surface coating at 60°C for 12 hours to ensure sufficient polymerization reaction and obtain a surface grafted polymer layer sufficient to form a breathing effect.
[0113] The reactive monomers of the polymer buffer layer are a mixed gas of acryl pyrrole and diacetone acrylamide vapor;
[0114] The conditions of the plasma device are:
[0115] Select a plasma enhanced chemical vapor deposition device, the RF power source should be set at 13.56 MHz, and the power should be adjusted to 500 watts to control the energy output of the plasma and ensure that the diacetone acrylamide can react evenly and completely during the polymerization process;
[0116] The ratio of acrylpyrrole and diacetone acrylamide vapor is controlled at 1:0.6;
[0117] Gas flow rates: The flow rate of acryloyl pyrrole was set at 100 sccm (standard cubic centimeters per minute), and the flow rate of diacetone acrylamide vapor was set at 60 sccm (standard cubic centimeters per minute).
[0118] Step 4: The interfacial buffer multilayer gradient composite film prepared in step 3 is cold pressed and composited with the lithium metal negative electrode at a pressure of 2 MPa for 20 seconds to form a protective layer of the multilayer gradient composite film on the surface of the lithium metal negative electrode, and the obtained modified negative electrode is stored in a vacuum.
[0119] Step 5: Assemble the modified negative electrode (including separator) prepared in step 4 with the positive electrode, solid-liquid mixed electrolyte, shell, etc. to form a semi-solid lithium metal battery; test the battery-related electrical properties and safety performance, and conduct a comprehensive evaluation of the battery.
[0120] Comparative Example 1
[0121] A semi-solid lithium metal battery was prepared using the same scheme as in Example 1, wherein the negative electrode was unmodified lithium metal; the other steps were the same.
[0122] Comparative Example 2
[0123] A semi-solid lithium metal battery was prepared using the same scheme as in Example 1, wherein the negative electrode was lithium metal modified by a composite membrane, but the composite membrane did not include the nanoporous polyamide layer prepared using the interfacial polymerization scheme in Example 1; the other steps were the same.
[0124] Comparative Example 3
[0125] A semi-solid lithium metal battery was prepared using the same scheme as in Example 1, wherein the negative electrode was lithium metal modified by a composite membrane, but the composite membrane did not include the breathing polymer buffer layer formed by grafting modification in Example 1; the other steps were the same.
[0126] Comparative Example 4
[0127] A semi-solid lithium metal battery was prepared using the same protocol as in Example 1, wherein acrylyl pyrrole was not added in step 3.
[0128] Comparative Example 5
[0129] A semi-solid lithium metal battery was prepared using the same protocol as in Example 1, wherein diacetone acrylamide was not added in step 3.
[0130] Comparative Example 6
[0131] The scheme of Example 6 is basically the same as that of Example 1, except that the reaction gas in step 3 contains only methyl methacrylate.
[0132] Test example:
[0133] The performance of the lithium batteries in Examples 1 to 5 and Comparative Examples 1 to 6 was tested respectively. Specifically, each lithium battery after formation was subjected to a cycle test, each lithium battery was charged at a constant current of 0.33C at 25°C to a voltage of 4.2 V, and then discharged at a constant current of 0.5C until the voltage reached 2.75V, and the aforementioned charge and discharge cycle was repeated 100 times, with a time interval of 10 min between two adjacent cycles, and the capacity retention rate after the cycle was calculated, and each lithium battery that completed the aforementioned cycle test was subjected to a national standard hot box and overcharge test. The test results are shown in Table 1 below:
[0134] Table 1
[0135] Example Cycle number / cycle capacity retention rate Overcharge test Hot box test Example 1 100 cycles 96.6% pass pass Example 2 100 cycles 95.7% pass pass Example 3 100 cycles 95.2% pass pass Example 4 100 cycles 94.8% pass pass Example 5 100 cycles 93.3% pass pass Comparative Example 1 5 cycles to failure Not passed Not passed Comparative Example 2 31 cycles to failure pass Not passed Comparative Example 3 100 cycles 81.3% pass pass Comparative Example 4 100 cycles 91.4% pass pass Comparative Example 5 100 cycles 90.7% pass pass Comparative Example 6 100 cycles 86.5% pass pass
[0136] It can be seen from the data results of the experimental tests that the method of the embodiment of the present application is applied to lithium batteries, which can alleviate the stress effect caused by the expansion and contraction of lithium metal batteries during charging and discharging, improve the compatibility of the electrolyte and lithium metal, make the lithium element deposit evenly, inhibit dendrite growth, maintain battery capacity stability, and improve battery safety and cycle performance.
[0137] The specific embodiments described herein are merely examples of the spirit of the present invention. A person skilled in the art of the present invention may make various modifications or additions to the specific embodiments described or replace them in a similar manner, but this will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. An interface buffer multilayer gradient composite film, characterized in that: It includes a multi-layer gradient composite membrane and a breathable polymer buffer layer chemically grafted on one side of the multi-layer gradient composite membrane; The multilayer gradient composite membrane comprises pore channels for transporting lithium ions, and the pore diameters of the pore channels increase in sequence in a direction away from the breathing polymer buffer layer; The quasi-breathable polymer buffer layer is composed of a comb-shaped polymer containing carbonyl groups; The multilayer gradient composite membrane is obtained by sequentially composite a polyamide membrane, a porous polyethylene membrane and a porous cellulose membrane; The quasi-breathing polymer buffer layer is chemically grafted onto the surface of the polyamide membrane.
2. The interface buffer multilayer gradient composite film according to claim 1, characterized in that: The comb polymer also contains pyrrole groups.
3. A method for preparing an interfacial buffer multilayer gradient composite film as claimed in any one of claims 1 or 2, characterized in that: The method comprises the steps of placing a multilayer gradient composite membrane in a plasma atmosphere, introducing vapor of a reaction monomer containing a carbonyl group therein, thereby grafting a comb-shaped polymer on the surface of the multilayer gradient composite membrane to obtain a breathing polymer buffer layer.
4. The method according to claim 3, characterized in that The reactive monomer is one or a combination of acrylic acid monomer, acrylamide monomer, methacrylic acid monomer, vinyl acetate monomer, acrylyl pyrrole, and diacetone acrylamide.
5. The method according to claim 4, characterized in that The reaction monomer is a mixed gas of acryl pyrrole and diacetone acrylamide vapor; wherein, The ratio of the acrylpyrrole to diacetone acrylamide vapor is 1:0.3-1:0.
6.
6. The method according to claim 3, characterized in that The preparation method of the multilayer gradient composite membrane is as follows: (S.1) hot-pressing a porous polyethylene stretched film and a porous cellulose film to obtain a double-layer composite film; (S.2) dissolving a diamine monomer in an aqueous solvent to obtain an aqueous reaction solution; dissolving the polyacyl chloride monomer in an oil phase organic solvent to obtain an oil phase reaction solution; (S.3) The double-layer composite membrane is immersed in an aqueous reaction solution and then taken out, so that a layer of aqueous reaction solution adheres to the surface of the double-layer composite membrane. The double-layer composite membrane is then immersed in an oil-phase reaction solution, so that the diamine monomer on the surface of the double-layer composite membrane reacts with the polyacyl chloride monomer to form a polyamide membrane, thereby obtaining a multi-layer gradient composite membrane.
7. The method according to claim 6, characterized in that The diamine monomer includes one or more of m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, xylylenediamine, ethylenediamine, propylenediamine, 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, piperazine, and 4-aminomethylpiperazine.
8. The method according to claim 6, characterized in that The polyacyl chloride monomer includes one or more of isophthaloyl chloride, terephthaloyl chloride, 1,3,5-trimesoyl chloride, and 9,10-anthraquinone-2-sulfonyl chloride.
9. A lithium metal battery, characterized in that: It comprises an interface buffer multilayer gradient composite film as described in any one of claims 1 or 2.