A zinc-magnesium-polyetheretherketone composite intervertebral fusion cage for intervertebral fusion

The zinc-magnesium-PEEK composite intervertebral fusion cage made of zinc-magnesium-polyetheretherketone composite material solves the deficiencies in biocompatibility and mechanical properties of existing intervertebral fusion materials and achieves closeness to natural bone tissue. The elastic modulus and compressive strength reduce implant risks and significantly improve biosafety and mineralization deposition rate.

CN118557789BActive Publication Date: 2024-10-18PEKING UNIVERSITY THIRD HOSPITAL (THE THIRD CLINICAL MEDICAL SCHOOL OF PEKING UNIVERSITY)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411026183.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-18
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

Existing intervertebral cage materials have deficiencies in biocompatibility, mechanical properties, degradation properties and biosafety, leading to risks of implant displacement, magnetic resonance imaging artifacts, inflammatory reactions, infection and secondary surgery. It is difficult to meet the needs of clinical treatment.

Method used

Using zinc-magnesium-polyetheretherketone composite material, through the combination of Zn3Mg alloy and PEEK shell, laser powder bed fusion technology is used to manufacture the wedge-shaped Zn3Mg alloy part, and it is fitted through mortise and tenon connection to form a near-natural bone tissue. Elastic modulus and compressive strength of composite interbody cages.

Benefits of technology

It improves the mechanical properties and biological safety of the implant, reduces the risk of late osteolysis and nerve compression, significantly increases the mineralization deposition rate at the interface with the end plate, and ensures the biocompatibility and degradation safety of the material. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118557789B_ABST
    Figure CN118557789B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of medical devices, and specifically relates to a zinc-magnesium-polyetheretherketone composite intervertebral fusion device for intervertebral fusion, which is composed of a Zn3Mg alloy part and a PEEK shell sleeved on the outside of the Zn3Mg alloy part. The Zn3Mg alloy part is manufactured by laser powder bed melting technology, with a porosity of 40% to 73%, an aperture of 400μm to 650μm, and an elastic modulus of the zinc-magnesium-polyetheretherketone composite intervertebral fusion device similar to that of natural bone tissue. The overall shape of the Zn3Mg alloy part is wedge-shaped, including a Zn3Mg alloy part body and a cylindrical hole running through the upper and lower surfaces of the Zn3Mg alloy part body, and the angle between one side of the Zn3Mg alloy part body and the axial midline of the cylindrical hole is 7 degrees. The outer layer of the present application is wrapped by PEEK material, which can effectively prevent the symptoms such as nerve compression caused by the inner alloy fragments entering the spinal canal.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of medical devices, and in particular relates to a zinc-magnesium-polyetheretherketone composite intervertebral fusion device for intervertebral fusion. Background Art

[0002] Degenerative disc disease is one of the common diseases in the field of orthopedics. Surgical treatment usually involves removing the damaged disc and implanting a specific fusion device to fill the gap caused by the removal to achieve the effect of postoperative support and prevent the collapse of the gap and instability. At present, according to the different materials of the implant, intervertebral fusion devices are mainly divided into metal, polymer, composite and absorbable fixation types, each with its own unique advantages and limitations.

[0003] Titanium alloy and polyetheretherketone (PEEK) are commonly used intervertebral fusion materials in clinical practice. Titanium alloy is widely used because of its excellent biocompatibility and ability to directly bond with bones. The calcium and phosphate surface layer it forms at the bone-implant interface helps to inhibit inflammatory response and promote the binding of osteoblasts. Although titanium alloy provides a high initial fixation strength, metal implants may have problems such as displacement and magnetic resonance imaging artifacts. In addition, due to its non-degradable properties, long-term presence of titanium alloy implants in the body may lead to complications such as infection and foreign body sensation, and may require secondary surgery to remove.

[0004] Organic polymer materials represented by PEEK have stable biological inertness, good postoperative imaging properties, and are not prone to acute inflammatory reactions. However, the hydrophobicity and inertness of PEEK limit its adhesion to proteins and cells, and its bone integration ability is relatively poor.

[0005] In addition, materials based on degradable polymers, such as poly(lactic acid), PLA, poly(glycolic acid), PGA, and hydroxyapatite, HA, and their copolymers, are available. These materials have mechanical properties close to those of cancellous bone and can be degraded in vivo, avoiding the need for secondary surgery. Nevertheless, polymer-based implants may increase the risk of surgical failure due to their insufficient strength or plasticity, and their degradation products may induce long-term inflammatory responses in surrounding tissues.

[0006] In recent years, biodegradable metal materials based on magnesium (Mg) and its alloys have received widespread attention. These materials have good biocompatibility, do not require secondary surgery for removal, and show obvious osteoinduction. However, the rapid degradation rate of Mg and the hydrogen produced may increase the risk of implant dislocation and fragmentation. In view of the limitations of magnesium alloys, researchers have begun to pay attention to zinc (Zn)-based materials with more stable chemical properties and slower degradation rates. Zinc is a trace element required by the human body, participates in a variety of physiological processes, and has good biosafety and osteoinduction. However, pure Zn in the cast state has certain cytotoxicity, low mechanical strength, and high brittleness. The fragmentation of the fusion cage will affect the stability of fixation and may cause persistent pain, inflammatory response, nerve compression, and even paralysis.

[0007] Therefore, comprehensively considering the biocompatibility, mechanical properties, degradation characteristics and biosafety of the materials, and finding new intervertebral fusion materials and their structural designs are of great significance for improving clinical treatment effects and reducing the risk of complications. Summary of the invention

[0008] The object of the present invention is to provide a zinc-magnesium-polyetheretherketone composite intervertebral fusion cage for intervertebral fusion to solve the problems existing in the above-mentioned background technology.

[0009] To achieve the above objectives, this application is implemented through the following technical solutions:

[0010] A zinc-magnesium-polyetheretherketone composite intervertebral fusion device for intervertebral fusion consists of a Zn3Mg alloy part and a PEEK shell sleeved on the outside of the Zn3Mg alloy part, wherein the number 3 in the Zn3Mg alloy part represents the weight percentage of zinc and magnesium.

[0011] Furthermore, the elastic modulus of the zinc-magnesium-polyetheretherketone composite intervertebral fusion device is 1.8 to 2.7 GPa, which is close to the elastic modulus of natural bone tissue.

[0012] Furthermore, the compression strength of the zinc-magnesium-polyetheretherketone composite intervertebral fusion device is 11.4 - 155.7 MPa.

[0013] Furthermore, the Zn3Mg alloy part is manufactured by laser powder bed fusion technology.

[0014] Furthermore, the Zn3Mg alloy part is wedge-shaped as a whole, including a Zn3Mg alloy part body and a cylindrical hole passing through the upper and lower surfaces of the Zn3Mg alloy part body, and an angle between a side surface of the Zn3Mg alloy part body and the axial centerline of the cylindrical hole is 5-10 degrees.

[0015] Furthermore, the porosity of the Zn3Mg alloy body is 40% to 73%, and the pore size is between 400 μm and 650 μm.

[0016] Furthermore, the Zn3Mg alloy body has a curved lattice structure.

[0017] Furthermore, the Zn3Mg alloy part and the PEEK shell are joined together by mortise and tenon rivets to form a zinc-magnesium-PEEK composite fusion device.

[0018] The beneficial effects of the present invention are:

[0019] 1. Mechanical advantage: Compared with titanium alloy intervertebral fusion devices, the mechanical property advantage of Zn3Mg-PEEK composite materials lies in the elastic modulus close to that of natural bone tissue, which can effectively reduce the osteolysis around the screws caused by the stress shielding effect of the material in the later stage; in addition, Zn3Mg alloy without PEEK wrapping is implanted in the body, and it will be broken or yielded, resulting in poor fusion with the end plate and loss of intervertebral disc height. The outer layer wrapped by PEEK material can effectively prevent the inner alloy fragments from entering the spinal canal to cause nerve compression and other symptoms.

[0020] 2. Biological safety: Since magnesium alloys produce H during degradation in the body 2 The pH of the local microenvironment was increased sharply, which is the main factor affecting its biosafety as an implant material; H&E staining results showed that no obvious immune rejection reaction and inflammatory cell infiltration were observed in the composite material group ( Figure 3 The venous blood collection results showed ( Figure 4 ), serum Zn in 12 weeks after implantation 2+ and Mg 2+ There was no significant difference in concentration compared with that before surgery, which further confirmed the good biocompatibility of Zn3Mg.

[0021] 3. Osteogenic mineralization ability: Calcein results showed that the mineralization deposition rate at the interface between Zn3Mg and the end plate was significantly higher than that of the titanium alloy group at 12 weeks ( Figure 5 ). BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 These are views of the composite intervertebral fusion cage of the present invention, wherein a is a top view, b is a side view, c is a front view, and d is a rear view.

[0023] Figure 2 This is a conceptual diagram of the composite intervertebral fusion device of the present invention.

[0024] Figure 3 This is the H&E staining image of the heart, liver, spleen, lung and kidney tissues of the group implanted with the composite intervertebral fusion device of the present invention 12 weeks after surgery. The scale bar represents 500 μm.

[0025] Figure 4 The composite intervertebral fusion device of the present invention was implanted before and 12 weeks after surgery, wherein Figure A shows the serum Zn 2+ Figure B shows the expression of Mg in serum 2+ expression of.

[0026] Figure 5 The composite intervertebral fusion device group of the present invention and the titanium alloy fusion device group were implanted 12 weeks after surgery, wherein Figure A is a calcein staining diagram, and Figure B is a semi-quantitative result comparison diagram. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is described in detail below through examples. The following examples are merely exemplary and can only be used to explain and illustrate the technical solution of the present invention, but cannot be construed as limiting the technical solution of the present invention.

[0028] like Figure 1 As shown, the zinc-magnesium-polyetheretherketone composite intervertebral fusion device for intervertebral fusion of the present application consists of a Zn3Mg alloy part and a PEEK shell sleeved on the outside of the Zn3Mg alloy part, wherein the number 3 in the Zn3Mg alloy part represents the weight percentage of zinc and magnesium.

[0029] The Zn3Mg alloy part of the present application is manufactured by laser powder bed fusion (LPBF) technology. The Zn3Mg alloy part is wedge-shaped as a whole, including a Zn3Mg alloy part body and a cylindrical hole penetrating the upper and lower surfaces of the Zn3Mg alloy part body, and the angle between one side of the Zn3Mg alloy part body and the axial center line of the cylindrical hole is 5-10 degrees, preferably 7 degrees. In the technical solution of the present application, the difference between different embodiments is only that the size will be slightly different, and the porosity and pore size of the Zn3Mg alloy part body will be different.

[0030] In this technical solution, if Figure 1 As shown, the diameter of the cylindrical holes on the upper and lower surfaces of the Zn3Mg alloy body is 3 mm. In this embodiment, the size of the composite intervertebral fusion device is 11×9×5.5 mm as an example for explanation. Of course, the size of the composite intervertebral fusion device used will vary depending on the height of different users, but it will not affect the implementation of the technical solution of the present application.

[0031] Among the mechanical properties of the composite intervertebral fusion device of the present application, the difference between its elastic modulus and that of natural bone is that the elastic modulus of the composite intervertebral integrator is similar to that of natural bone tissue. The Zn3Mg alloy body of the present application has a minimal curved surface lattice structure, a porosity of 40% to 73%, and a pore size of 400μm to 650μm. The outer surface of the Zn3Mg alloy body and the PEEK shell with an outer thickness of 1mm are joined by mortise and tenon joints to form a zinc-magnesium-PEEK composite fusion device.

[0032] Compared with titanium alloy intervertebral fusion devices, the advantage of the mechanical properties of Zn3Mg-PEEK composite materials lies in the elastic modulus that is close to that of natural bone tissue. The elastic modulus of this application ranges from 1.8 to 2.7 GPa, and the compressive strength is 11.4 - 155.7 Mpa, which can effectively reduce the bone dissolution around the screws caused by the stress shielding effect of the material in the later stage; in addition, Zn3Mg alloy without PEEK wrapping is implanted in the body, and fragmentation or yield deformation occurs, resulting in poor fusion with the end plate and loss of intervertebral disc height, while the outer layer wrapped by PEEK material can effectively prevent the inner alloy fragments from entering the spinal canal and causing symptoms such as nerve compression.

[0033] Since magnesium alloys produce H during degradation in the body 2 The pH of the local microenvironment was increased sharply, which is the main factor affecting its biosafety as an implant material; H&E staining results showed that no obvious immune rejection reaction and inflammatory cell infiltration were observed in the composite material group ( Figure 3 The venous blood collection results showed ( Figure 4 ), serum Zn in 12 weeks after implantation 2+ and Mg 2+ There was no significant difference in concentration compared with that before surgery, which further confirmed the good biocompatibility of Zn3Mg. The results of calcein showed that the mineralization deposition rate of the interface between Zn3Mg and the end plate was significantly higher than that of the titanium alloy group at 12 weeks ( Figure 5 ).

[0034] Test Example 1

[0035] Surgical model construction:

[0036] The sheep cervical motion segment is considered to be an ideal experimental model for simulating the human cervical motion segment due to its biomechanical similarity. Eight male small-tailed Han sheep (1 year old, about 50 kg) were selected to undergo anterior cervical decompression and fusion at the C3 / 4 and C4 / 5 intervertebral spaces. The specific surgical steps are as follows.

[0037] (1) Fast for 24 hours before surgery. Anesthesia is induced by intramuscular injection of midazolam combined with sodium pentobarbital solution. After endotracheal intubation, isoflurane is inhaled by a ventilator to maintain the depth of anesthesia. After anesthesia is successfully implemented, the patient lies in a supine position with a pillow under the neck and shoulders to hyperextend the neck. Routine iodine and alcohol disinfection is performed, and a drape is laid.

[0038] (2) Make a longitudinal incision 1 cm lateral to the right side of the trachea along the anterior neck and 10 to 25 cm below the lower edge of the cricoid cartilage, and cut the skin and subcutaneous tissue layer by layer.

[0039] (3) Incise the deep and superficial cervical fascia along the inner edge of the pectoralis major muscle. Use a thyroid retractor to pull the omohyoid muscle apart, paying attention to protecting the esophagus and trachea. Bluntly separate along the medial side of the common carotid artery to the anterior part of the vertebra, insert a Kirschner wire into the intervertebral space, and confirm the C3 / 4 or 4 / 5 intervertebral space with C-arm fluoroscopy.

[0040] (4) Cut the longus colli muscle along the midline at its anterior attachment to the C3-5 vertebral body, separate the longus colli muscle to both sides, peel off the prevertebral fascia and anterior longitudinal ligament, and expose the anterior part of the C3-5 vertebral body.

[0041] (5) Use a 11# knife to remove the C3 / 4 intervertebral disc, screw two traction screws into the C3 and C4 vertebrae, place an intervertebral spacer, and open the intervertebral disc. Use a scraper, nucleus pulposus forceps, etc. to remove the intervertebral disc and expose the posterior longitudinal ligament. Use an endplate scraper to remove the adjacent vertebral cartilage to the endplate.

[0042] (6) Take a suitable intervertebral fusion cage, expand it appropriately, and insert the cage between the C3 / 4 and C4 / 5 vertebrae.

[0043] (7) Remove the spacer and see that the fusion cage is stable. Remove the traction pins of the intervertebral spacer.

[0044] (8) Titanium plate was implanted at C3-5. Anteroposterior and lateral fluoroscopy confirmed that the position and depth of the fusion device and internal fixation were satisfactory. The locking screws were tightened.

[0045] (9) Rinse the wound, perform strict bipolar hemostasis, and close the anterior cervical incision layer by layer after checking the gauze and instruments to make sure they are correct.

[0046] One week after the experiment, the animals were allowed to eat freely without additional fixation or activity restriction of the cervical spine. Blood was collected from the ear vein before and 12 weeks after the operation for serological testing. Twelve weeks after the operation, the experimental animals were killed with an overdose of diazepam and KCl, and the corresponding spinal segments were taken for subsequent analysis, and heart, liver, spleen, lung, and kidney tissues were taken for biosafety assessment.

[0047] Test Example 2

[0048] Histological staining:

[0049] (1) Immediately after the experimental animals were killed, the heart, liver, spleen, lung, and kidney tissues were removed and fixed in 4% paraformaldehyde for 48 hours.

[0050] (2) Place the specimen in an embedding box, mark it, rinse it in running water for 2 hours, and then dehydrate it.

[0051] (3) Dehydration steps: 50% ethanol soak for 1 h, 80% ethanol soak for 1 h, 95% ethanol soak for 1 h, 100% ethanol soak for 1.5 h, xylene soak for 1 h, paraffin soak for 1 h.

[0052] (4) After dehydration, routine embedding, sectioning, and dewaxing are performed.

[0053] (5) Ethanol gradient hydration: 100%, 95%, 90%, 80%, 70%, and 60% ethanol solutions for 5 min each.

[0054] (6) Soak in distilled water for a total of 3 min × 2 times, and soak in PBS for 5 min.

[0055] (7) After staining with hematoxylin for 60 seconds, wash off the stain.

[0056] (8) Separate with 1% hydrochloric acid and ethanol for 3 minutes and wash with water for 3 seconds.

[0057] (9) Debluing with 0.5% ammonia water for 10 seconds, and washing with water for 30 seconds.

[0058] (10) Stain with eosin solution for 30 seconds and wash with distilled water for 10 seconds.

[0059] (11) Gradient dehydration in ethanol solution: 70%, 80%, 90%, and 100% ethanol for 2 seconds each.

[0060] (12) Xylene substitute transparency: Xylene substitutes (I) and (II) for 1 min each.

[0061] (13) After sealing with neutral resin, the slides were air-dried in a fume hood for one week before images were acquired using a slide scanner.

[0062] Test Example 3

[0063] Zn in serum 2+ and Mg 2+ Concentration detection:

[0064] Serum samples obtained before and 12 weeks after surgery were sent to the Peking University Analysis and Testing Center for determination of Zn 2+ Mg 2+ The concentrations of the two ions in the extract, such as Figure 4 shown.

[0065] Test Example 4

[0066] Observation of new bone tissue at fusion interface by fluorescence staining:

[0067] 5 mg / kg calcein and 100 mg / kg xylenol orange fluorescent dye were subcutaneously injected 10 and 20 days before each small-tail Han sheep was killed to mark the new bone tissue; hard tissue sections were observed using a confocal microscope. Figure 5 Shown: Calcein (488nm) - green, xylenol orange (543nm) - red represents new bone. The distance between dye markers was divided by the number of days between markers to calculate the mineral apposition rate (MAR). Five samples were calculated in each group, and the average of three areas in each sample was taken.

[0068] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A zinc-magnesium-polyetheretherketone composite intervertebral fusion cage for intervertebral fusion, characterized in that: It consists of a Zn3Mg alloy part and a PEEK shell covered on the outside of the Zn3Mg alloy part, wherein the number 3 in the Zn3Mg alloy part represents the weight percentage of zinc and magnesium; The Zn3Mg alloy portion is wedge-shaped as a whole, including a Zn3Mg alloy portion body and a cylindrical hole passing through the upper and lower surfaces of the Zn3Mg alloy portion body; The Zn3Mg alloy body has a curved lattice structure; The Zn3Mg alloy part and the PEEK shell are joined together by mortise and tenon riveting to form a zinc-magnesium-PEEK composite fusion device.

2. The zinc-magnesium-polyetheretherketone composite intervertebral fusion cage for intervertebral fusion according to claim 1, characterized in that: The elastic modulus of the zinc-magnesium-polyetheretherketone composite intervertebral fusion device is 1.8-2.7 GPa, which is close to the elastic modulus of natural bone tissue.

3. The zinc-magnesium-polyetheretherketone composite intervertebral fusion cage for intervertebral fusion according to claim 1, characterized in that: The compressive strength of the zinc-magnesium-polyetheretherketone composite intervertebral fusion cage is 11.4-155.7 MPa.

4. The zinc-magnesium-polyetheretherketone composite intervertebral fusion cage for intervertebral fusion according to claim 1, characterized in that: The Zn3Mg alloy part is manufactured using laser powder bed fusion technology.

5. The zinc-magnesium-polyetheretherketone composite intervertebral fusion cage for intervertebral fusion according to claim 1, characterized in that: An angle between one side surface of the Zn3Mg alloy body and the axial center line of the cylindrical hole is 5-10 degrees.

6. The zinc-magnesium-polyetheretherketone composite intervertebral fusion cage for intervertebral fusion according to claim 5, characterized in that: The porosity of the Zn3Mg alloy body is 40% to 73%, and the pore diameter is between 400 μm and 650 μm.