Piezoelectric polyaryletherketone bone repair scaffold as well as preparation method and application thereof

By adding nanobarium titanate and nanohydroxyapatite to the bone repair material, and using 3D printing technology to prepare piezoelectric polyaryl etherketone bone repair scaffolds, the problem of bone defect morphology diversity is solved, and personalized customization is achieved and Improved biocompatibility promotes bone regeneration and cell proliferation, and solves the stress shielding and cytotoxicity problems of barium titanate ceramics.

CN118949128APending Publication Date: 2024-11-15DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES

Patent Information

Application Number
CN202410993868.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Existing bone repair materials are difficult to meet the specific bone defect morphology and structure caused by different reasons, and have high biological inertia. In addition, simple barium titanate ceramics will cause stress shielding when bone defect repair, making it difficult to heal, and Restricted by the cytotoxicity of barium.

Method used

Provide an ultrasonic-responsive piezoelectric polyaryl etherketone bone repair scaffold, prepared by 3D printing, adding nanobarium titanate and nanohydroxyapatite to form multi-stage micropores from nano-scale to micro-scale, improving biocompatibility and mechanical strength, and promote cell proliferation and differentiation under low-intensity ultrasound.

Benefits of technology

A personalized customized bone repair scaffold is realized, which promotes cell adhesion and bone regeneration, provides long-term and stable electrical stimulation, improves the proliferation and differentiation of bone-forming cells, reduces biological inertia, and enhances the biocompatibility and mechanical properties of the scaffold. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949128A_ABST
    Figure CN118949128A_ABST
Patent Text Reader

Abstract

The invention discloses a piezoelectric polyaryletherketone bone repair scaffold as well as a preparation method and application thereof, and belongs to the technical field of medical biological materials. The piezoelectric polyaryletherketone bone repair scaffold is prepared from a mixture containing amorphous polyaryletherketone, nano barium titanate and nano hydroxyapatite through 3D printing. According to the piezoelectric polyaryletherketone bone repair scaffold provided by the invention, mechanical energy can be converted into electric energy at a bone defect part by simulating the inherent piezoelectric effect of a natural bone, and long-term and stable electrical stimulation is provided. The electrical stimulation plays an important role in growth and remodeling of bones, and can promote proliferation and differentiation of cells in vivo and in vitro.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a piezoelectric polyaryletherketone bone repair scaffold and a preparation method and application thereof, belonging to the technical field of medical biomaterials. Background Art

[0002] Bone defects caused by trauma, tumors, infection, and functional atrophy have become one of the main problems that seriously affect the limb function of patients and cause physical and mental harm. At present, the use of bone tissue engineering scaffold materials can provide a microenvironment for bone regeneration and is an effective alternative strategy to support bone regeneration. Among the various biomaterials used for bone tissue engineering, high-performance resin polyaryletherketone (PEEK, PEKK) has good biocompatibility, low cytotoxicity, stable physical and chemical properties, and good radiotransparency. In the 1990s, it gradually replaced metal and became a new choice for orthopedic implants (ColloidsSurf B Biointerfaces.2021,111726). In recent years, the preparation of multi-level controllable porous scaffolds by low-temperature solution 3D printing technology has shown good bone integration effects in vitro and in vivo. However, traditional polyaryletherketones are semi-crystalline, insoluble in organic solvents, and difficult to perform low-temperature solution 3D printing. For this reason, phenolphthalein-based poly(aryletherketone), which has similar properties to traditional poly(aryletherketone) and is the most representative amorphous form, is considered to be an ideal low-temperature 3D printed high-performance orthopedic implant (CN116262825A).

[0003] In addition, a variety of emerging studies have found that various physiological cues, including mechanical, electrical, and magnetic stimulation, represent new prospects for bone repair by affecting cell fate and participating in the biological process of bone regeneration. It is well known that electrical signals play a vital role in bone formation and fracture healing. Natural bone tissue is known to be piezoelectric, so piezoelectric materials are promising in implants because they can convert mechanical forces into electrical signals, enabling them to provide electrical stimulation to surrounding bone tissue without surgical implantation of electrodes. As the first piezoelectric ceramic reported for bone regeneration research, barium titanate has received widespread attention as a lead-free ceramic implant material with good biocompatibility (Small.2023, e2206401). Studies have shown that composite materials containing barium titanate can have a positive effect on the proliferation, migration, and differentiation of bone-forming cells (CN117658662A, CN116942901A). However, pure barium titanate ceramics have a high elastic modulus, which causes stress shielding when used for bone defect repair, ultimately leading to difficulty in healing fractures. And due to the cytotoxicity of barium, it is necessary to prepare it into a composite material through special methods before using it for bone regeneration and repair. Summary of the invention

[0004] In view of the fact that existing bone repair materials are difficult to meet various specific bone defect morphologies and structures caused by different reasons and have high biological inertness, the present application provides an ultrasonically responsive piezoelectric polyaryletherketone bone repair scaffold with good bone regeneration and repair promotion, as well as its preparation method and application. The piezoelectric polyaryletherketone bone repair scaffold not only has a personalized customized structure and shape, but also has multi-level micropores from nanoscale to micron scale obtained by solvent volatilization, which can well promote cell adhesion. More importantly, the addition of nano-hydroxyapatite and nano-barium titanate can well improve the biological inertness of the scaffold, enhance the performance of the scaffold so that it has bone-like mechanical strength, piezoelectric effect and biocompatibility. And under the action of low-intensity ultrasound, the piezoelectric effect of barium titanate can further promote cell proliferation, differentiation and adhesion.

[0005] According to one aspect of the present application, a piezoelectric polyaryletherketone bone repair scaffold is provided, wherein the piezoelectric polyaryletherketone bone repair scaffold is made of a mixture containing amorphous polyaryletherketone, nano-barium titanate and nano-hydroxyapatite by 3D printing;

[0006] The amorphous polyaryletherketone is selected from at least one of the structures shown in Formula I-1, Formula I-2, and Formula I-3;

[0007]

[0008]

[0009] Wherein, in formula I-1, the value of n is 80 to 160;

[0010] In formula I-2, the value of n1 is 80 to 160;

[0011] In formula I-3, the value of m is 40 to 80, and the value of n2 is 40 to 80.

[0012] Optionally, in formula I-1, the value of n is independently selected from any value among 80, 90, 100, 110, 120, 130, 140, 150, 160 or a range between any two of the above.

[0013] Optionally, in formula I-2, the value of n1 is independently selected from any value among 80, 90, 100, 110, 120, 130, 140, 150, 160 or a range between any two of the above values.

[0014] Optionally, in formula I-3, the value of m is independently selected from any value of 40, 45, 50, 55, 60, 65, 70, 75, 80 or a range between any two of the above values.

[0015] Optionally, in formula I-3, the value of n2 is independently selected from any value of 40, 45, 50, 55, 60, 65, 70, 75, 80 or a range between any two of the above values.

[0016] Optionally, the number average molecular weight of the amorphous polyaryletherketone is 4.0×10 4 ~8.0×10 4 g / mol.

[0017] Optionally, the number average molecular weight of the amorphous polyaryletherketone is independently selected from 4.0×10 4 g / mol, 4.5×10 4 g / mol, 5.0×10 4 g / mol, 5.5×10 4 g / mol, 6.0×10 4 g / mol, 6.5×10 4 g / mol, 7.0×10 4 g / mol, 7.5×10 4 g / mol, 8.0×10 4 g / mol or any range between the above two values.

[0018] Optionally, the porosity of the piezoelectric polyaryletherketone bone repair scaffold is 40-60%.

[0019] Optionally, the porosity of the piezoelectric polyaryletherketone bone repair scaffold is independently selected from any value of 40%, 45%, 50%, 55%, 60% or a range between any two of the above values.

[0020] According to another aspect of the present application, a method for preparing a piezoelectric polyaryletherketone bone repair scaffold is provided, the preparation method comprising the following steps: using a mixed solution containing amorphous polyaryletherketone, nano-barium titanate and nano-hydroxyapatite to prepare a bone tissue engineering scaffold by 3D printing, pre-freezing, and vacuum freeze-drying to obtain a piezoelectric polyaryletherketone bone repair scaffold with multi-level pores.

[0021] Optionally, the mass fraction of amorphous polyaryletherketone in the mixed solution is 10% to 30%.

[0022] Optionally, the mass fraction of amorphous polyaryletherketone in the mixed solution is independently selected from any value of 10%, 12%, 15%, 20%, 25%, 30% or a range between any two of the above.

[0023] Optionally, the mass fraction of nano-barium titanate in the mixed solution is 2% to 20%.

[0024] Optionally, the mass fraction of nano-barium titanate in the mixed solution is independently selected from any value among 2%, 5%, 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20% or a range between any two of the above.

[0025] Optionally, the mass fraction of nano-hydroxyapatite in the mixed solution is 10% to 20%.

[0026] Optionally, the mass fraction of nano-hydroxyapatite in the mixed solution is independently selected from any value of 10%, 12%, 14%, 15%, 16%, 18%, 20% or a range between any two of the above.

[0027] Optionally, the solvent in the mixed solution is selected from at least one of 1,4-dioxane and dimethyl sulfoxide.

[0028] Optionally, the parameters of the 3D printing are: nozzle temperature is 15°C to 25°C; extrusion air pressure is 0.4MPa to 0.6MPa; platform temperature is -20°C to -10°C; printing speed is 4mm / s to 6mm / s; filling spacing is 0.7mm to 0.9mm; printing corner direction is [0°, 90°]; and the filling method is linear filling.

[0029] Optionally, the pre-freezing temperature is -196°C to -20°C.

[0030] Optionally, the pre-freezing temperature is independently selected from any value among -196°C, -190°C, -180°C, -150°C, -140°C, -120°C, -100°C, -80°C, -60°C, -50°C, -40°C, -20°C or a range between any two of the above.

[0031] Optionally, the pre-freezing time is 5 to 10 hours.

[0032] Optionally, the pre-freezing time is independently selected from any value among 5h, 6h, 7h, 8h, 9h, 10h or a range value between any two of the above.

[0033] Optionally, the vacuum freeze-drying temperature is -60°C to -30°C.

[0034] Optionally, the vacuum freeze-drying temperature is independently selected from any value among -60°C, -55°C, -50°C, -45°C, -40°C, -35°C, -30°C or a range between any two of the above.

[0035] Optionally, the vacuum freeze-drying time is 12h to 24h.

[0036] Optionally, the vacuum freeze-drying time is independently selected from any value among 12h, 14h, 16h, 18h, 20h, 22h, 24h or a range between any two of the above.

[0037] Optionally, as a specific implementation method, the present application is implemented through the following technical solutions:

[0038] S1: Establish customized bone defect implant models of various shapes according to the patient's specific bone defect shape and anatomical structure, and use software to design a three-dimensional model in STL format with ideal porosity and pore size;

[0039] S2: dissolving amorphous poly(aryletherketone) powder in 1,4-dioxane solvent to prepare solutions with different relative mass fractions, and subjecting to ultrasonic treatment for 2 hours to fully dissolve the solutions;

[0040] S3: Weigh corresponding masses of nano-barium titanate and nano-hydroxyapatite powder, and add them into the solution prepared in step S2 by physical blending and ultrasonic mixing to obtain bio-inks with different mass fractions;

[0041] S4: Using the STL format model in the low-temperature solution 3D printer to fix the bio-ink on the low-temperature deposition platform to prepare a bone tissue engineering scaffold of a predetermined shape;

[0042] S5: Pre-freeze various bone tissue engineering scaffolds in liquid nitrogen, and then freeze-dry them in a freeze dryer under vacuum to obtain a piezoelectric polyaryletherketone bone repair material with multi-level pores.

[0043] Optionally, in step S5, the freeze dryer is pre-cooled to -30°C.

[0044] Optionally, in step S5, the various bone tissue engineering scaffolds prepared can be subjected to vacuum freeze-drying to volatilize the solvent and form multi-level micropores of nanometer to micrometer scale on the surface of the material to promote cell adhesion.

[0045] In the present application, the molecular structure of amorphous polyaryletherketone is as follows:

[0046] Amorphous poly(aryletherketone) containing phenolphthalein, abbreviated as "PEK-C";

[0047] Amorphous poly(aryletherketone) containing pendant carboxyl groups, abbreviated as "PEK-COOH";

[0048] Isosorbide-based amorphous polyaryletherketone, abbreviated as "PIEK".

[0049] According to another aspect of the present application, there is provided an application of the piezoelectric polyaryletherketone bone repair scaffold or the piezoelectric polyaryletherketone bone repair scaffold prepared by the above preparation method in promoting cell growth and osteogenic differentiation.

[0050] Optionally, the piezoelectric properties are stimulated by means of in vitro ultrasound to promote osteogenesis.

[0051] Optionally, the ultrasonic parameters are: frequency of 0.7 MHz to 1.3 MHz; intensity of 20 mW / cm 2 ~40mW / cm 2 ; Pulse width is 1ms~2ms; pulse repetition frequency is 80Hz~120Hz.

[0052] Optionally, the ultrasonic frequency is independently selected from any value among 0.7 MHz, 0.8 MHz, 0.9 MHz, 1.0 MHz, 1.1 MHz, 1.2 MHz, 1.3 MHz or a range between any two of the above.

[0053] Optionally, the ultrasound intensity is independently selected from 20 mW / cm 2 、22mW / cm 2 , 24mW / cm 2 、26mW / cm 2 、28mW / cm 2 、30mW / cm 2 、32mW / cm 2 、34mW / cm 2 、36mW / cm 2 、38mW / cm 2 、40mW / cm 2 Any value in or a range between any two of the above.

[0054] Optionally, the ultrasonic pulse width is independently selected from any value among 1 ms, 1.1 ms, 1.2 ms, 1.3 ms, 1.4 ms, 1.5 ms, 1.6 ms, 1.7 ms, 1.8 ms, 1.9 ms, 2 ms, or a range between any two of the above.

[0055] Optionally, the ultrasound pulse repetition frequency is independently selected from any value of 80 Hz, 85 Hz, 90 Hz, 95 Hz, 100 Hz, 105 Hz, 110 Hz, 115 Hz, 120 Hz or a range between any two of the above values.

[0056] The beneficial effects of this application include:

[0057] (1) The piezoelectric polyaryletherketone bone repair scaffold provided in the present application utilizes its solution-processable characteristics to dissolve it in an organic solvent, and the prepared bio-ink is then formed by low-temperature 3D printing. Compared with the traditional polyaryletherketone melt processing method, low-temperature 3D printing can accurately control the porosity and pore size of the scaffold, and can effectively avoid the inactivation of the incorporated bioactive substances caused by high temperature. In addition, the low-temperature 3D printed scaffold can form multi-level pores from nanometers to micrometers on the surface of the scaffold through the volatilization of the solvent to promote cell adhesion.

[0058] (2) The piezoelectric polyaryletherketone bone repair scaffold provided in this application can convert mechanical energy into electrical energy at the bone defect site by simulating the inherent piezoelectric effect of natural bone, providing long-term and stable electrical stimulation. This electrical stimulation plays an important role in bone growth and remodeling, and can promote cell proliferation and differentiation in vivo and in vitro.

[0059] (3) The piezoelectric polyaryletherketone bone repair scaffold provided in this application has good physical, chemical and biological properties and good in vivo safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 Actual pictures of piezoelectric polyaryletherketone bone repair scaffolds with different contents of nano-barium titanate and nano-hydroxyapatite prepared in Comparative Examples 1-2 and Examples 1-2 of the present application.

[0061] Figure 2 Fourier transform infrared spectra and X-ray diffraction patterns of the piezoelectric polyaryletherketone bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 of the present application.

[0062] Figure 3 The electron microscope images and energy spectrum images of the piezoelectric polyaryletherketone bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 of the present application.

[0063] Figure 4 These are the piezoelectric effect test results of the piezoelectric polyaryletherketone bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 of the present application.

[0064] Figure 5 These are the in vitro biosafety test results of the piezoelectric polyaryletherketone bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 of the present application.

[0065] Figure 6 These are the cell live-dead staining results of the piezoelectric poly(aryletherketone) bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 of the present application. DETAILED DESCRIPTION

[0066] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.

[0067] Unless otherwise specified, the raw materials and solvents in the examples of the present application were purchased through commercial channels.

[0068] The analysis method in the examples of this application is as follows:

[0069] The 3D printer manufacturer is Hangzhou GeneFluid Biotech Co., Ltd. and the model is REGENOVO.

[0070] The infrared spectrometer IRTrace-100 produced by Shimadzu Corporation of Japan was used to obtain a resolution of 4 cm -1 , scanning range is 500~2000cm -1 , cumulative scan 128, and infrared spectrum analysis was performed.

[0071] The XRD test and analysis were performed using an X-ray diffractometer (XRD) device manufactured by Rigaku Corporation of Japan, which scanned the sample in the range of 10° to 80° at a speed of 5° / min.

[0072] The surface microstructure and energy spectrum analysis of the composite stent with gold spraying treatment were carried out using the scanning electron microscope JSM-7800F manufactured by Czech Tasken (Shanghai) Co., Ltd.

[0073] The Keithley 6517B device from Cleveland, USA, was used to impact the material at a mechanical frequency of 1s / time and the output current and voltage of the bracket were recorded.

[0074] The CCK-8 reagent and cell viability test kit produced by Shanghai Bio-Tech Biotechnology Co., Ltd. were used to perform in vitro biosafety testing on the composite scaffolds co-cultured with cells.

[0075] Comparative Example 1

[0076] A preparation method of a piezoelectric polyaryletherketone bone repair scaffold is provided, comprising the following steps:

[0077] (1) Preparation of 3D printing bio-ink: Weigh 3 g of a 3D printing bio-ink with a number average molecular weight of approximately 4 × 10 4 The phenolphthalein-based amorphous poly(aryletherketone) (PEK-C) powder of 100 g / mol was dissolved in 7 ml of 1,4-dioxane solvent to prepare a 30% mass fraction solution, and ultrasonically vibrated for 2 hours to completely dissolve it.

[0078] (2) Design of 3D printing model: The porosity of the scaffold was designed to be 40-60%, the layer height was 0.2 mm, and the shapes were 15×3 mm, 5×6 mm cylinders, and 10×10×10 mm cubes. The generated STL format digital model was imported into the 3D printer.

[0079] (3) Preparation of piezoelectric bone tissue engineering scaffolds: The 3D printing parameters were set as follows: nozzle temperature was 15°C to 25°C, extrusion pressure was 0.4 MPa to 0.6 MPa, low temperature platform temperature was -10°C to -20°C, printing speed was 4 mm / s to 6 mm / s, filling spacing was 0.9 mm, printing angle direction was [0°, 90°], and filling method was linear filling.

[0080] (4) Freeze-drying of piezoelectric bone tissue engineering scaffolds: The scaffolds were pre-frozen in liquid nitrogen for 5 to 10 hours, and then freeze-dried for 12 to 24 hours in a freeze dryer that had been pre-cooled to -30°C under vacuum and -60°C conditions to obtain a piezoelectric poly(aryletherketone) bone repair scaffold, denoted as P.

[0081] Comparative Example 2

[0082] On the basis of comparative example 1, without changing other conditions, 10% of nanohydroxyapatite by mass was weighed and dissolved in the 3D printing bio-ink prepared in step (1) by physical blending, and ultrasonicated for 2 to 3 hours. The remaining steps were the same to obtain a piezoelectric polyaryletherketone bone repair scaffold, which was recorded as PH.

[0083] Example 1

[0084] On the basis of comparative example 1, without changing other conditions, 10% of nano-hydroxyapatite and 5% of nano-barium titanate were weighed and dissolved in the 3D printing bio-ink prepared in step (1) by physical blending, and ultrasonicated for 2 to 3 hours. The remaining steps were the same to obtain a piezoelectric polyaryletherketone bone repair scaffold, which was recorded as PH5B.

[0085] Example 2

[0086] On the basis of comparative example 1, without changing other conditions, 10% of nano-hydroxyapatite and 10% of nano-barium titanate were weighed and dissolved in the 3D printing bio-ink prepared in step (1) by physical blending, and ultrasonicated for 2 to 3 hours. The remaining steps were the same to obtain a piezoelectric polyaryletherketone bone repair scaffold, which was recorded as PH10B.

[0087] The actual pictures of the piezoelectric polyaryletherketone bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 are as follows: Figure 1 As shown by Figure 1 It can be seen that the piezoelectric polyaryletherketone bone repair scaffold has good three-dimensional connectivity and controllable pore size. The scaffold has a diameter of about 15 mm, a height of about 3 mm, and a porosity of about 60%.

[0088] The piezoelectric polyaryletherketone bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 were subjected to X-ray diffraction and FTIR tests. The test results are shown in Figure 2 , which can be seen at 618cm in Figure a -1The characteristic peak of Ti-O bond is observed at Figure 2 Figure b shows the characteristic peaks of nano-hydroxyapatite at 26° and 31.7° and the characteristic peak of nano-barium titanate at about 45.4°. Figure 2 It can be seen that the piezoelectric polyaryletherketone bone repair scaffolds prepared from nano-hydroxyapatite and micron-sized barium titanate powders in different proportions will not change in their phase structures after printing.

[0089] The scanning electron microscope images and energy spectrum of the piezoelectric polyaryletherketone bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 are as follows: Figure 3 As shown by Figure 3 It can be seen that no incompatibility of inorganic fillers was found in the piezoelectric polyaryletherketone bone repair scaffold, and each component was evenly dispersed.

[0090] The piezoelectric effect test of the piezoelectric poly(aryletherketone) bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 was performed using an electrometer. The test results are shown in Figure 4 , Figure 4 Figure a shows the magnitude of the current generated by the composite bracket subjected to mechanical impact. Figure 4 Figure b in the middle shows the magnitude of the pressure generated by the composite bracket subjected to mechanical impact. Figure 4 It can be seen that the doping of nano-scale barium titanate can obviously introduce piezoelectric properties into the system, and as the content increases, the power generation capacity increases. And the doping of nano-hydroxyapatite will not affect its piezoelectric properties.

[0091] The piezoelectric polyaryletherketone bone repair scaffolds prepared in Examples 1 to 2 and Examples 1 to 2 were subjected to in vitro biosafety testing using low-intensity ultrasound stimulation. The test results are shown in Figure 5 , Figure 5 Figure a in the middle shows the CCK-8 test results of cells after co-culture of cells and scaffolds for 3 days. Figure 5 Figure b shows the CCK-8 test results of cells after 5 days of co-culture. The OD value is positively correlated with the number of cells, which directly reflects the biocompatibility of the scaffold. Figure 5 It can be seen that the addition of nano-hydroxyapatite and nano-barium titanate will not inhibit cell proliferation, and each group has no cytotoxicity.

[0092] The piezoelectric polyaryletherketone bone repair scaffolds prepared in Comparative Examples 1-2 and Examples 1-2 were directly co-cultured with cells and then subjected to live-dead staining. The test results are shown in Figure 6 This further verifies the safety and effectiveness of piezoelectric polyaryletherketone bone repair scaffolds.

[0093] Example 3

[0094] On the basis of Example 2, without changing other conditions, the phenolphthalein-containing amorphous poly(aryletherketone) (PEK-C) was replaced with a poly(aryletherketone) having a number average molecular weight of about 4×104 The piezoelectric poly(aryletherketone) bone repair scaffold prepared by the method of Example 2 has a similar effect to that of Example 2.

[0095] Example 4

[0096] On the basis of Example 2, without changing other conditions, the phenolphthalein-containing amorphous poly(aryletherketone) (PEK-C) was replaced with a poly(aryletherketone) having a number average molecular weight of about 4×10 4 g / mol isosorbide-based amorphous poly(aryletherketone) (PIEK), the effect of the prepared piezoelectric poly(aryletherketone) bone repair scaffold is similar to that in Example 2.

[0097] Unless otherwise specified, all numbers appearing in the specification and claims of this application, such as temperature, time, conversion rate, etc., should not be understood as absolutely precise values. Due to the standard deviation of the measurement technology, the measured values ​​inevitably have certain experimental errors.

[0098] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A piezoelectric polyaryletherketone bone repair scaffold, characterized in that: The piezoelectric polyaryletherketone bone repair scaffold is prepared by 3D printing from a mixture of amorphous polyaryletherketone, nano-barium titanate and nano-hydroxyapatite; The amorphous polyaryletherketone is selected from at least one of the structures shown in Formula I-1, Formula I-2, and Formula I-3; Wherein, in formula I-1, the value of n is 80 to 160; In formula I-2, the value of n1 is 80 to 160; In formula I-3, the value of m is 40 to 80, and the value of n2 is 40 to 80.

2. The piezoelectric polyaryletherketone bone repair scaffold according to claim 1, characterized in that: The number average molecular weight of the amorphous polyaryletherketone is 4.0×10 4 ~8.0×10 4 g / mol; Preferably, the porosity of the piezoelectric polyaryletherketone bone repair scaffold is 40-60%.

3. A method for preparing the piezoelectric polyaryletherketone bone repair scaffold according to any one of claims 1 to 2, characterized in that: The preparation method comprises the following steps: using a mixed solution containing amorphous polyaryletherketone, nano-barium titanate and nano-hydroxyapatite to prepare a bone tissue engineering scaffold by 3D printing, pre-freezing, and vacuum freeze-drying to obtain a piezoelectric polyaryletherketone bone repair scaffold with multi-level pores.

4. The preparation method according to claim 3, characterized in that: The mass fraction of amorphous polyaryletherketone in the mixed solution is 10% to 30%; The mass fraction of nano-barium titanate in the mixed solution is 2% to 20%; The mass fraction of nano-hydroxyapatite in the mixed solution is 10% to 20%.

5. The preparation method according to claim 3, characterized in that: The solvent in the mixed solution is selected from at least one of 1,4-dioxane and dimethyl sulfoxide.

6. The preparation method according to claim 3, characterized in that: The parameters of the 3D printing are: The temperature of the nozzle is 15℃~25℃; The extrusion pressure is 0.4MPa~0.6MPa; The platform temperature is -20℃~-10℃; Printing speed is 4mm / s~6mm / s; Filling spacing 0.7mm~0.9mm; Print the corner direction [0°, 90°]; The filling method is linear filling.

7. The preparation method according to claim 3, characterized in that: The pre-freezing temperature is -196°C to -20°C; The pre-freezing time is 5 to 10 hours.

8. The preparation method according to claim 3, characterized in that: The vacuum freeze-drying temperature is -60°C to -30°C; The vacuum freeze-drying time is 12h to 24h.

9. Use of the piezoelectric polyaryletherketone bone repair scaffold according to any one of claims 1 to 2 or the piezoelectric polyaryletherketone bone repair scaffold prepared by the preparation method according to any one of claims 3 to 8 in promoting cell growth and osteogenic differentiation.

10. The use according to claim 9, characterized in that: Stimulate piezoelectric properties by ultrasound in vitro to promote osteogenesis; Preferably, the ultrasonic parameters are: The frequency is 0.7MHz~1.3MHz; Intensity: 20mW / cm 2 ~40mW / cm 2 ; The pulse width is 1ms to 2ms; The pulse repetition frequency is 80Hz~120Hz.

Citation Information

Patent Citations

  • Polyaryletherketone bone repair material and preparation method thereof

    CN116262825A

  • Bone repair material as well as preparation method and application thereof

    CN116942901A

  • Ultrasonic response immunoregulation piezoelectric ceramic bone scaffold and preparation method thereof

    CN117658662A

Cited By

  • White calcium stone-polyethylene glycol-polylactic acid shape memory polymer, preparation method thereof and application of white calcium stone-polyethylene glycol-polylactic acid shape memory polymer in preparation of bone repair scaffold

    CN119875333A