Titanium alloy artificial bone joint with low friction coefficient and preparation method thereof
By adopting specific proportional materials and multi-layer structural design in titanium alloy artificial bone joints, combined with advanced preparation technology, the shortcomings of titanium alloy artificial bone joints in terms of mechanical properties, biocompatibility and low friction coefficient are solved, which is significantly Improves its performance and service life.
Patent Information
- Application Number
- CN202411035183.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The existing titanium alloy artificial bone joints have significant defects in mechanical properties, biocompatibility and low coefficient of friction, resulting in material fatigue, inflammatory response and joint wear, limiting their service life and clinical applications.
Using titanium alloy materials containing a specific weight ratio, the combination of matrix structure, fusion layer, intermediate layer and surface layer is designed, combined with vapor deposition method and spraying process, improve the mechanical properties and biocompatibility of the material and reduce the friction coefficient. .
It significantly improves the tensile strength, yield strength and biocompatibility of titanium alloy artificial bone joints, reduces the friction coefficient, extends the service life of the joint and improves the comfort of the patient.
Smart Images

Figure CN118948500A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bone joints, in particular to an artificial bone joint of a titanium alloy with a low friction coefficient and a preparation method thereof. Background Art
[0002] The research and development and application of artificial bone joints is one of the important directions in the field of modern medicine. Especially in orthopedic surgery, the application of artificial joints has greatly improved the quality of life of patients. Titanium alloy has become an important material for the preparation of artificial bone joints due to its good mechanical properties, biocompatibility and corrosion resistance. However, existing titanium alloy artificial bone joints still have some significant defects in mechanical properties, biocompatibility and low friction coefficient.
[0003] Titanium alloy has high strength and low density, which makes it one of the ideal artificial bone joint materials. However, existing titanium alloy artificial bone joints often suffer from fatigue damage and wear problems during long-term use. Since human joints are subjected to repeated stress and strain in daily activities, artificial joint materials are required to have excellent tensile strength and yield strength. The performance of existing titanium alloy artificial bone joints in this regard is not ideal. Long-term use may cause the mechanical properties of the material to deteriorate, affecting the service life and function of the joints.
[0004] Biocompatibility is one of the important indicators for evaluating the quality of artificial bone and joint materials. Although the existing titanium alloy artificial bone and joints generally show good biocompatibility after being implanted in the human body, there are still some problems. For example, some titanium alloy materials may induce local inflammatory reactions, leading to tissue rejection of the implant. In addition, the existing titanium alloy surface treatment technology is limited, and it is difficult to achieve good integration with the surrounding bone tissue, affecting bone healing and the long-term stability of the joint. The cytotoxicity problem also limits the widespread application of existing titanium alloy artificial bone and joints to a certain extent.
[0005] The normal functioning of joints depends on low friction and high lubricity between the joint surfaces. Existing titanium alloy artificial bone joints still perform unsatisfactorily in this regard. The high coefficient of friction of titanium alloys means that during joint movement, friction and wear will increase, thus affecting the function and durability of the joint. The high coefficient of friction will not only cause discomfort to patients during use, but may also cause wear and inflammation of the tissues around the joints, further reducing the service life of the artificial joints.
[0006] In summary, existing titanium alloy artificial bone joints have a large room for improvement in mechanical properties, biocompatibility and low friction coefficient. These defects limit the widespread application and promotion of artificial bone joints in clinical practice. In view of these problems, it is particularly important to develop a titanium alloy artificial bone joint with higher mechanical properties, better biocompatibility and lower friction coefficient. Summary of the invention
[0007] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a titanium alloy artificial bone joint with a low friction coefficient and a preparation method thereof, which significantly improves the mechanical properties, biocompatibility and low friction coefficient of the titanium alloy artificial bone joint, overcomes the deficiencies in the prior art, and provides a better solution for the clinical application of artificial bone joints.
[0008] The technical solution adopted by the present invention to achieve the above-mentioned purpose is: a titanium alloy artificial bone joint with a low friction coefficient, including a joint part and a padding structure arranged at the connection between adjacent joint parts, the joint part includes an action part and a connecting part, the action part is matched with the padding structure, and the connecting part is fixedly connected to the natural bone or artificial bone.
[0009] The action part and the connection part both include a base structure arranged on the inner side, the action part also includes an intermediate layer attached to the outer side of the base structure and a surface layer attached to the outer side of the intermediate layer; the connection part also includes a fusion layer attached to the outer side of the base structure.
[0010] In some of the implementations, in order to ensure that the matrix structure in the action part and the connecting part exhibits excellent mechanical properties, the following technical solutions are provided.
[0011] The matrix structure comprises the following raw material components in proportion by weight:
[0012] Titanium: ≥85%,
[0013] Nitrogen: 5-10%,
[0014] Aluminum: 2-8%,
[0015] Vanadium: 1-2%.
[0016] In some of the implementations, in order to further improve the structural strength, biocompatibility, processing performance and corrosion resistance of the matrix structure, the following technical solutions are provided.
[0017] The matrix structure also includes the following raw material components in proportion by weight:
[0018] Iron: ≤0.25%,
[0019] Zirconium: ≤0.3%,
[0020] Molybdenum: ≤1.5%.
[0021] In some of the implementations, in order to ensure that the fusion layer can stably adhere to the base structure of the connection part to form a unified whole, ensure that the fusion layer has good biocompatibility and can achieve effective fusion with natural bone, and improve the stability of the combination of artificial bone joints and natural bones, the following technical solutions are provided.
[0022] The fusion layer comprises the following raw material components in proportion by weight:
[0023] Titanium: 85-90%,
[0024] Bioactive glass: 10-15%;
[0025] The bioactive glass comprises the following raw material components in proportion by weight:
[0026] Silicon dioxide: 45-52%,
[0027] Calcium oxide: 25-30%,
[0028] Sodium oxide: 10-15%,
[0029] Phosphorus oxide: 2-6%.
[0030] In some of the implementations, the following technical solutions are provided to enable the intermediate layer to be stably attached and bonded to the base structure of the active part to form a unified whole, while further improving the strength and rigidity of the entire active part, enhancing its impact and fatigue resistance, ensuring long-term stable use, and playing the role of bearing and dispersing stress.
[0031] The middle layer is evenly provided with anchor holes on one side facing the liner structure, and the middle layer comprises the following raw material components in proportion by weight:
[0032] Titanium: 85-95%,
[0033] Tantalum: 5-10%,
[0034] Niobium: 1-5%,
[0035] Ceramic matrix composite materials: ≤5%;
[0036] The ceramic matrix composite material comprises the following raw material components in proportion by weight:
[0037] Alumina: 70-80%,
[0038] Zirconia: 20-30%,
[0039] Additives: ≤5%;
[0040] The additives include one or more of silicon dioxide, titanium oxide, and rare earth oxides.
[0041] In some of the implementations, in order to ensure that the surface layer can stably adhere to the outer surface of the middle layer and form a unified whole, while ensuring that the surface layer has an extremely low friction coefficient and operates smoothly in coordination with the liner structure, the following technical solutions are provided.
[0042] The surface layer adopts a nitrogen-containing high-carbon nanocrystalline titanium alloy coating, and the nitrogen-containing high-carbon nanocrystalline titanium alloy coating includes the following raw material components in proportion by weight:
[0043] Nanocrystalline titanium: ≥80%,
[0044] Nitrogen: 4-8%,
[0045] Charcoal: 2-5%.
[0046] In some of the implementations, in order to reduce the friction between the lining structure and the surface layer of the action part, the following technical solutions are provided.
[0047] The liner structure comprises the following raw material components in proportion by weight:
[0048] PEEK: 90-95%,
[0049] Tetrafluoroethylene fiber: 5-10%.
[0050] A method for preparing a titanium alloy artificial bone joint with a low friction coefficient is used to prepare the titanium alloy artificial bone joint with a low friction coefficient mentioned above, and includes the following steps for preparing the joint part:
[0051] S1-1. Preparation of matrix structure:
[0052] S1-1-1: preparing a blank by a melt casting method;
[0053] S1-1-2: The surface of the blank is subjected to cutting and finishing, polishing of the edges and corners, sandblasting, and cleaning in sequence to obtain a base structure showing a connecting portion and an action portion;
[0054] S1-2. Preparation of fusion layer:
[0055] S1-2-1: coating the base structure of the action part, installing a coating shell on the outside of the action part, and forming a fusion layer on the outer surface of the base structure of the connection part by a vapor deposition method;
[0056] S1-2-2: removing the outer covering shell of the action part and cleaning the base structure of the action part;
[0057] S1-3. Preparation of the middle layer:
[0058] S1-3-1: coating the fusion layer of the connection part, adding a coating shell to the outside of the fusion layer, and using a vapor deposition method to make an intermediate layer on the outer surface of the base structure of the action part;
[0059] S1-3-2: Drill a hole on the side of the middle layer facing the cushion structure to form the anchor hole, and use a spraying process to make a surface layer on the outer surface of the middle layer so that the surface layer enters the anchor hole to enhance the bonding stability between the surface layer and the middle layer.
[0060] S1-3-3: removing the outer covering shell of the fusion layer and cleaning the entire joint component to complete the preparation of the joint component;
[0061] The preparation steps of the liner structure are also included:
[0062] S2: The one-piece cushion structure is processed by melt casting.
[0063] In some of the implementations, in order to ensure that the base structure of the active part and the fusion layer of the connecting part are coated to ensure that the vapor deposition operation of the exposed part is carried out stably, the following technical solutions are provided.
[0064] The coating shell is made of high temperature resistant material, and the coating treatment and removal of the coating shell include:
[0065] S3-1: The covering shell is detachably mounted on the outer side of the base structure of the action part or the outer side of the fusion layer of the connection part;
[0066] S3-2: Remove the outer covering shell of the base structure of the action part or the outer covering shell of the fusion layer of the connection part.
[0067] Beneficial effects of the present invention:
[0068] 1. This application prepares titanium alloy billets by melt casting and performs fine processing on them, such as cutting, polishing and sandblasting, so that the matrix structure has higher smoothness and geometric accuracy, laying a solid foundation for the subsequent attachment of the fusion layer and the intermediate layer. The preparation of the fusion layer and the intermediate layer adopts the vapor deposition method, which not only enhances the structural strength of the material, but also significantly improves the tensile strength and yield strength. The experimental results show that the tensile strength of the titanium alloy artificial bone joint provided in this application reaches 950MPa, and the yield strength reaches 920MPa, which are significantly better than the existing 850MPa and 800MPa. The improvement of the overall mechanical properties ensures the stability and durability of the joint in long-term use.
[0069] In terms of biocompatibility, the present application significantly reduces cytotoxicity by preparing a low-toxic fusion layer and an intermediate layer on the surface of the titanium alloy, and the cell proliferation rate reaches 95%. The surface treatment process of the present application makes the titanium alloy material more closely integrated with the surrounding bone tissue, reducing the risk of inflammatory response and tissue rejection. Through cell culture experiments, it is verified that the titanium alloy artificial bone joint provided by the present application shows obvious advantages in biocompatibility, which is conducive to the healing of bone tissue and the long-term stability of artificial joints.
[0070] 3. The present application uses a spraying process to prepare a nitrogen-containing high-carbon nanocrystalline coating on the titanium alloy surface, and drills anchor holes on the middle layer to allow the surface layer material to enter the anchor holes, thereby enhancing the bonding stability between the surface layer and the middle layer. After friction and wear tests, the friction coefficient of the titanium alloy artificial bone joint provided by the present application is only 0.20, which is significantly lower than the 0.35 of the existing titanium alloy artificial bone joint. The realization of a low friction coefficient not only reduces wear and energy consumption during joint movement, but also improves the patient's comfort and the service life of the joint.
[0071] In summary, this application significantly improves the mechanical properties, biocompatibility and low friction coefficient of titanium alloy artificial bone joints through innovative preparation methods and surface treatment processes, overcomes the shortcomings of the existing technology, and provides a better solution for the clinical application of artificial bone joints. BRIEF DESCRIPTION OF THE DRAWINGS
[0072] Figure 1 It is a schematic diagram of the structure of the titanium alloy bone joint in the present invention in a cut state;
[0073] Figure 2 This is a schematic diagram of the structure when the middle layer and the surface layer are disassembled.
[0074] In the figure: 1 joint part, 101 action part, 102 connection part, 11 base structure, 12 middle layer, 121 anchor hole, 13 surface layer, 14 fusion layer, 2 cushion structure. DETAILED DESCRIPTION
[0075] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0076] See also Figure 1-2 In combination with the following embodiments, the various technical solutions and working mechanisms of the titanium alloy artificial bone joint with a low friction coefficient and the preparation method thereof provided by the present invention are described in detail.
[0077] Example 1
[0078] A titanium alloy artificial bone joint with a low friction coefficient comprises a joint component 1 and a liner structure 2 arranged at the connection between adjacent joint components 1. The joint component 1 comprises an action part 101 and a connection part 102. The action part 101 is matched with the liner structure 2, and the connection part 102 is fixedly connected to the natural bone or artificial bone.
[0079] Both the action part 101 and the connection part 102 include a base structure 11 arranged on the inner side. The action part 101 also includes an intermediate layer 12 adhered to the outer side of the base structure 11 and a surface layer 13 adhered to the outer side of the intermediate layer 12 ; the connection part 102 also includes a fusion layer 14 adhered to the outer side of the base structure 11 .
[0080] The titanium alloy artificial bone joint with low friction coefficient provided by the present invention is reasonably designed, and the coordination between the various structures involved is strong, and each function can be fully exerted. Specifically:
[0081] The joint component 1 includes an action portion 101 and a connection portion 102, which have distinct functions. The action portion 101 cooperates with the cushion structure 2 to provide a low-friction surface required for joint movement, while the connection portion 102 is fixedly connected to the natural bone or artificial bone to provide stable support for the joint.
[0082] In the structural design of the action part 101, the base structure 11 provides structural support, bears the main load, has good mechanical properties, and ensures the stability of its own structure during joint movement; the middle layer 12 can further improve the strength and rigidity of the entire action part 101, enhance its impact and fatigue resistance, ensure long-term stable use, and play a role in bearing and dispersing stress, ensuring that the base structure 11, the surface layer 13 and the middle layer 12 can be stably bonded together to form an integral structure, avoiding problems such as delamination and cracking, and extending the service life of the joint; the surface layer 13 has an extremely low friction coefficient and excellent wear resistance, and directly acts on the lining structure 2 to achieve the effect of joint movement.
[0083] In the structural design of the connecting part 102, its base structure 11 is the same as the base structure 11 in the action part 101, and also has good compatibility with human bone tissue, ensuring that the connecting part 102 can be stably connected to the natural bone; the fusion layer 14 can further increase the good fusion with the natural bone or artificial bone, ensure a firm connection, and avoid loosening.
[0084] The pad structure 2 is arranged at the connection between adjacent joint parts 1 to buffer the impact force generated during joint movement, reduce stress concentration, protect the joint and surrounding tissues, and cooperate with the action part 101 to further optimize the low friction characteristics of the joint.
[0085] The design of each structure is based on key goals such as reducing friction, dispersing stress, and improving stability. Through mutual cooperation, the long-term stability and reliable operation of the artificial joint can be achieved.
[0086] Example 2
[0087] In order to ensure that the base structure 11 in the action part 101 and the connection part 102 presents excellent mechanical properties, the following technical solution is provided.
[0088] The matrix structure 11 includes the following raw material components in proportion by weight:
[0089] Titanium: ≥85%,
[0090] Nitrogen: 5-10%,
[0091] Aluminum: 2-8%,
[0092] Vanadium: 1-2%.
[0093] Among the titanium alloy components used in the base structure 11, titanium, as the main component, has good biocompatibility and mechanical properties, and nitrides can improve the hardness and wear resistance of the metal, and also improve the compatibility with human tissues. Aluminum can improve the strength and hardness of the titanium alloy and ensure its mechanical properties, and vanadium can improve the corrosion resistance of the titanium alloy on the basis of improving its strength.
[0094] In order to further improve the structural strength, biocompatibility, processing performance and corrosion resistance of the base structure 11, the following technical solutions are provided.
[0095] The matrix structure 11 also includes the following raw material components in proportion by weight:
[0096] Iron: ≤0.25%,
[0097] Zirconium: ≤0.3%,
[0098] Molybdenum: ≤1.5%.
[0099] Iron can be added selectively to improve the heat treatment performance of titanium alloys while increasing their strength; zirconium can also be added selectively to improve the processing performance and biocompatibility of titanium alloys; molybdenum can be added selectively to improve the corrosion resistance and strength of titanium alloys.
[0100] Example 3
[0101] In order to ensure that the fusion layer 14 can be stably attached to the base structure 11 of the connection part 102 to form a unified whole, ensure that the fusion layer 14 has good biocompatibility and can achieve effective fusion with natural bones, and improve the combination stability of artificial bone joints and natural bones, the following technical solutions are provided.
[0102] The fusion layer 14 includes the following raw material components in proportion by weight:
[0103] Titanium: 85-90%,
[0104] Bioactive glass: 10-15%;
[0105] Bioactive glass includes the following raw material components in proportion by weight:
[0106] Silicon dioxide: 45-52%,
[0107] Calcium oxide: 25-30%,
[0108] Sodium oxide: 10-15%,
[0109] Phosphorus oxide: 2-6%.
[0110] Silica is a network former of bioactive glass, which gives bioactive glass good mechanical strength and chemical stability. In the body, silica can hydrolyze to release Si ions, stimulate surrounding cells to produce silicate and phosphate precipitation, and promote the formation of new bone tissue.
[0111] Calcium oxide can increase the bioactivity and dissolution rate of bioactive glass. The release of calcium ions is beneficial to cell adhesion and proliferation, and it can also combine with phosphate ions to form hydroxyapatite, forming a chemical bond with natural bone.
[0112] Sodium oxide can regulate the dissolution rate of glass to maintain appropriate bioactive reaction kinetics in vivo. The release of sodium ions helps extracellular matrix mineralization and new bone formation.
[0113] Phosphorus oxide can further enhance the bioactivity of bioactive glass and promote the formation of hydroxyapatite. At the same time, the release of phosphate ions is beneficial to cell differentiation and bone mineralization process.
[0114] The components of the bioactive glass will undergo a series of complex chemical-biological reactions in the body, which together promote the regeneration and fusion of bone tissue. After the addition of titanium, the fusion layer 14 can be stably attached to the outer surface of the base structure 11 to form a unified whole.
[0115] Example 4
[0116] In order to enable the intermediate layer 12 to stably adhere to the base structure 11 of the active part 101 to form a unified whole, and at the same time further improve the strength and rigidity of the entire active part 101, enhance its impact resistance and fatigue resistance, ensure long-term stable use, and play a role in bearing and dispersing stress, the following technical solution is provided.
[0117] The middle layer 12 is evenly provided with anchor holes 121 on one side facing the liner structure 2. The middle layer 12 includes the following raw material components in proportion by weight:
[0118] Titanium: 85-95%,
[0119] Tantalum: 5-10%,
[0120] Niobium: 1-5%,
[0121] Ceramic matrix composite materials: ≤5%;
[0122] The ceramic matrix composite material includes the following raw material components in proportion by weight:
[0123] Alumina: 70-80%,
[0124] Zirconia: 20-30%,
[0125] Additives: ≤5%;
[0126] The additives include one or more of silicon dioxide, titanium oxide, and rare earth oxides.
[0127] Titanium, as the main component, has excellent properties such as high strength, light weight and corrosion resistance. Tantalum is a metal element with high density, corrosion resistance and good biocompatibility. Adding tantalum to titanium alloy can improve the strength, hardness and wear resistance of the alloy. Niobium is a metal element with good biocompatibility, which can improve the mechanical properties of the alloy. Adding an appropriate amount of niobium to titanium alloy can increase the strength, toughness and fatigue resistance of the alloy, and also help improve the corrosion resistance of the alloy, ensuring the long-term stability of joint prostheses in physiological environments.
[0128] Alumina is a high-strength, high-hardness ceramic material that can significantly improve the mechanical strength and stiffness of composite materials. It has excellent wear resistance and corrosion resistance, can significantly enhance the durability of composite materials, and has good thermal stability at high temperatures, which is conducive to improving the fatigue resistance of composite materials.
[0129] Zirconia has high fracture toughness, can effectively inhibit crack expansion, and improve the impact resistance of the composite material. Volume expansion during phase change can generate compressive stress, prevent crack propagation, and enhance wear resistance. When an anchor hole 121 is opened on the side of the intermediate layer 12 facing the liner structure 2, cracking around the anchor hole 121 can be effectively avoided. The chemical stability of zirconium oxide also helps to improve the durability of the composite material in the biological environment.
[0130] As for additives, silicon dioxide can improve the density and strength of ceramics, titanium oxide can improve the thermal shock resistance and wear resistance of ceramics, and rare earth oxides (such as yttrium oxide) can improve the fracture toughness and creep resistance of ceramics.
[0131] The anchor holes 121 can improve the effective adhesion and bonding of the surface layer 13 to the outer surface of the middle layer 12, improve the bonding effect of the two, ensure that the middle layer 12 and the surface layer 13 can be stably bonded together to form an integral structure, and avoid problems such as delamination and cracking.
[0132] In order to ensure that the surface layer 13 can be stably attached to the outer surface of the middle layer 12 and form a unified whole, and at the same time ensure that the surface layer 13 has an extremely low friction coefficient and operates smoothly in cooperation with the liner structure 2, the following technical solution is provided.
[0133] The surface layer 13 is a nitrogen-containing high-carbon nanocrystalline titanium alloy coating, which includes the following raw material components in proportion by weight:
[0134] Nanocrystalline titanium: ≥80%,
[0135] Nitrogen: 4-8%,
[0136] Charcoal: 2-5%.
[0137] The nanoscale grain size of nanocrystalline titanium can significantly improve the hardness and strength of the titanium alloy, thereby enhancing the wear resistance of the surface layer 13 . The nanocrystalline structure can also improve the thermal stability and chemical stability of the material, which is beneficial to improving the durability of the surface layer 13 .
[0138] The nitrogen element can form a TiN phase in the nanocrystalline titanium matrix, further improving the hardness and wear resistance of the surface layer 13 . The presence of the TiN phase can also improve the lubrication performance of the surface layer 13 and reduce the friction coefficient with the corresponding pad structure 2 .
[0139] Carbon elements can form TiC phase in nanocrystalline titanium, further enhancing the strength and toughness of the surface layer 13. The presence of the TiC phase can also improve the chemical stability of the surface layer 13, and enhance the corrosion resistance and wear resistance.
[0140] On this basis, other trace elements, specifically a small amount of Al, V, Fe and other elements, can be added to further optimize the performance of the surface layer 13, such as improving corrosion resistance and oxidation resistance.
[0141] During the bonding process of the surface layer 13 and the middle layer 12, part of the surface layer 13 material can penetrate into the anchor hole 121 of the middle layer 12 to form a stable anchoring structure to enhance the stability and unity of the combination of the two.
[0142] Example 5
[0143] In order to reduce the friction between the lining structure 2 and the surface layer 13 of the action part 101, the following technical solution is provided.
[0144] The liner structure 2 includes the following raw material components in proportion by weight:
[0145] PEEK: 90-95%,
[0146] Tetrafluoroethylene fiber: 5-10%.
[0147] Polyetheretherketone (PEEK) is a high-performance engineering plastic with excellent mechanical strength, rigidity and high temperature resistance. Its good chemical resistance and biocompatibility can ensure the stability and safety of the liner structure 2 in the biological environment, and its low friction coefficient and excellent self-lubrication are conducive to achieving low-friction movement with the surface layer 13.
[0148] Tetrafluoroethylene (PTFE) fiber has an extremely low friction coefficient and excellent wear resistance, which can further reduce the friction coefficient with the surface layer 13. In addition, the addition of PTFE fiber can also enhance the crack resistance of the PEEK matrix and improve the overall reliability and durability. The synergistic effect between PTFE fiber and PEEK matrix can achieve more stable low friction characteristics.
[0149] The PEEK matrix provides excellent mechanical strength and rigidity to withstand the high loads during joint movement.
[0150] Example 6
[0151] A method for preparing a titanium alloy artificial bone joint with a low friction coefficient is used to prepare the titanium alloy artificial bone joint with a low friction coefficient mentioned above, and includes the following steps for preparing a joint component 1:
[0152] S1-1, preparation of base structure 11:
[0153] S1-1-1: preparing a blank by a melt casting method;
[0154] S1-1-2: The surface of the blank is subjected to cutting and finishing, polishing of the edges and corners, sandblasting, and cleaning in sequence to obtain a base structure 11 having a connecting portion 102 and an action portion 101;
[0155] S1-2, Preparation of Fusion Layer 14:
[0156] S1-2-1: coating the base structure 11 of the action part 101, installing a coating shell on the outside of the action part 101, and forming a fusion layer 14 on the outer surface of the base structure 11 of the connection part 102 by a vapor deposition method;
[0157] S1-2-2: removing the outer covering shell of the action part 101 and cleaning the base structure 11 of the action part 101;
[0158] S1-3. Preparation of the intermediate layer 12:
[0159] S1-3-1: coating the fusion layer 14 of the connection part 102, installing a coating shell outside the fusion layer 14, and forming an intermediate layer 12 on the outer surface of the base structure 11 of the action part 101 by a vapor deposition method;
[0160] S1-3-2: Drill a hole in the middle layer 12 on one side facing the cushion structure 2 to form an anchor hole 121, and use a spraying process to make a surface layer 13 on the outer surface of the middle layer 12, so that the surface layer 13 enters the anchor hole 121 to enhance the bonding stability between the surface layer 13 and the middle layer 12.
[0161] S1-3-3: removing the outer covering shell of the fusion layer 14 and cleaning the entire joint component 1 to complete the preparation of the joint component 1;
[0162] The method also includes the following steps for preparing the liner structure 2:
[0163] S2: An integrally formed cushion structure 2 is produced by melt casting.
[0164] A titanium alloy billet is prepared by a melt casting method, which lays the foundation for subsequent processing. The billet is cut and finished to form the structure of the working part 101 and the connecting part 102. The edges and corners are then polished to remove impurities and burrs. Finally, the overall structure is sprayed to roughen the surface to facilitate the stable attachment of the fusion layer 14 and the intermediate layer 12 thereon to form a unified whole.
[0165] When generating the molten layer, the active part 101 is first coated by a coating method to prevent the molten layer material from falling on the active part 101 and affecting the structural stability of the active part 101. A fusion layer 14 is prepared on the surface of the substrate of the connecting part 102 by a vapor deposition method. Then, the coating shell on the outside of the active part 101 is removed, and the coating shell remaining on the surface of the substrate is cleaned.
[0166] When generating the intermediate layer 12, the fusion layer 14 is first coated by a coating method to prevent the materials of the intermediate layer 12 and the surface layer 13 from falling on the fusion layer 14 and affecting the normal performance of its design functions. The intermediate layer 12 is prepared by vapor deposition to improve the overall structural strength. Anchor holes 121 are drilled in the intermediate layer 12 to improve the bonding effect between the intermediate layer 12 and the surface layer 13, and the surface layer 13 is prepared by a spraying process so that it enters the anchor holes 121 to enhance the bonding. Finally, the coating shell on the outside of the connecting part 102 is removed, and the entire joint component 1 is cleaned to remove surface impurities.
[0167] The liner structure 2 is prepared by melt casting to form an integrally formed composite material liner structure 2 .
[0168] The fusion layer 14 and the intermediate layer 12 are prepared by a vapor deposition method, so that stable adhesion on the surface of the substrate can be achieved.
[0169] Cutting, polishing, sandblasting and other finishing processes can ensure the surface finish and geometric accuracy of the substrate, laying the foundation for the subsequent preparation of the adhesion layer. This series of surface treatment processes is conducive to improving the bonding force between the substrate structure 11 and the adhesion layer.
[0170] The spraying of the surface layer 13 and the design of the anchor hole 121 can prepare a low-friction nitrogen-containing high-carbon nanocrystalline coating on the surface of the intermediate layer 12. The anchor hole 121 is drilled on the intermediate layer 12 to allow the surface layer 13 material to enter therein, thereby enhancing the bonding stability between the two.
[0171] In order to ensure that the base structure 11 of the action part 101 and the fusion layer 14 of the connection part 102 are coated to ensure that the vapor deposition operation of the exposed part is carried out stably, the following technical solution is provided.
[0172] The coating shell is made of high temperature resistant material, and the steps of coating treatment and removal of the coating shell include:
[0173] S3-1: The covering shell is detachably mounted on the outer side of the base structure 11 of the action part 101 or the outer side of the fusion layer 14 of the connection part 102;
[0174] S3-2: The outer covering shell of the base structure 11 of the action part 101 or the outer covering shell of the fusion layer 14 of the connection part 102 is removed.
[0175] The protective shell is installed in a detachable manner, which can effectively protect the internal structure and facilitate its removal to perform vapor deposition on the internal structure and prepare the outer structure.
[0176] Example 7
[0177] In order to verify the superiority of the low friction coefficient titanium alloy artificial bone joint in the scheme of the present invention in terms of mechanical properties, biocompatibility and low friction coefficient, the following comparative experiment was designed to conduct detailed tests on the existing titanium alloy artificial bone joint and the artificial bone joint provided by the present application. The specific experimental process, i.e., the test data, is as follows:
[0178] Group A samples: Common titanium alloy artificial bone joints on the market were used as control group samples.
[0179] Group B samples: using a titanium alloy artificial bone joint with a low friction coefficient provided by the present invention, wherein:
[0180] The matrix structure includes the following raw material components in proportion by weight:
[0181] Titanium: 85%, Nitrogen: 6%, Aluminum: 5%, Vanadium: 2%, Iron: 0.25%, Zirconium: ≤0.25%, Molybdenum: 1.5%.
[0182] The fusion layer includes the following raw material components in proportion by weight:
[0183] Titanium: 85%, bioactive glass: 15%;
[0184] The bioactive glass includes the following raw material components in proportion by weight:
[0185] Silicon dioxide: 50%, calcium oxide: 30%, sodium oxide: 15%, phosphorus oxide: 5%.
[0186] The middle layer includes the following raw material components in proportion by weight:
[0187] Titanium: 90%, Tantalum: 5%, Niobium: 3%, Ceramic Matrix Composite: 2%.
[0188] The ceramic matrix composite material includes the following raw material components in proportion by weight:
[0189] Alumina: 75%, zirconium oxide: 20%, additive: 5%. The additive is silicon dioxide.
[0190] The surface layer adopts nitrogen-containing high-carbon nanocrystalline titanium alloy coating, and the nitrogen-containing high-carbon nanocrystalline titanium alloy coating includes the following raw material components in proportion by weight:
[0191] Nanocrystalline titanium: 90%, nitrogen: 7%, carbon: 3%.
[0192] The liner structure includes the following raw material components in proportion by weight:
[0193] Polyetheretherketone: 90%, tetrafluoroethylene fiber: 10%.
[0194] The complete joint component and the liner structure are processed according to the preparation method provided in Example 6.
[0195] The following experiments were performed on samples in group A and group B:
[0196] 1. Mechanical properties test: A universal testing machine was used to test the tensile strength, yield strength and hardness of the two titanium alloy artificial bone joints.
[0197] 2. Biocompatibility test: The in vitro cell culture method was used to evaluate the cytotoxicity and cell proliferation of the two titanium alloy artificial bone joints.
[0198] 3. Low friction coefficient test: The friction coefficient of two titanium alloy artificial bone joints was tested using a friction and wear testing machine.
[0199] Compare the test data of group A samples and group B samples:
[0200]
[0201]
[0202] Analysis of the test data of group A samples and group B samples:
[0203] 1. Mechanical properties:
[0204] The tensile strength of the titanium alloy artificial bone joint provided in the present application is 950 MPa, which is about 12% higher than the existing 850 MPa.
[0205] The yield strength of the titanium alloy artificial bone joint provided in the present application is 920 MPa, which is about 15% higher than the existing 800 MPa.
[0206] The hardness of the titanium alloy artificial bone joint provided in the present application is 380HV, which is about 19% higher than the existing 320HV.
[0207] 2. Biocompatibility:
[0208] The titanium alloy artificial bone joint provided in the present application exhibits low toxicity in a cytotoxicity test, while the existing titanium alloy artificial bone joint exhibits moderate toxicity.
[0209] In terms of cell proliferation rate, the titanium alloy artificial bone joint provided in this application is 95%, which is about 27% higher than the existing 75%.
[0210] 3. Low friction coefficient:
[0211] The friction coefficient of the titanium alloy artificial bone joint provided in the present application is 0.20, which is significantly lower than 0.35 of the existing titanium alloy artificial bone joint, a reduction of about 43%.
[0212] 4. Conclusion:
[0213] It can be seen from the above comparative experiments that the low-friction titanium alloy artificial bone joint provided by the present application is superior to the existing titanium alloy artificial bone joint in terms of mechanical properties, biocompatibility and low friction coefficient, reflecting the significant advantages of the present application scheme.
[0214] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0215] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A titanium alloy artificial bone joint with a low friction coefficient, characterized in that: The invention comprises a joint component (1) and a liner structure (2) arranged at the connection between adjacent joint components (1), wherein the joint component (1) comprises an action portion (101) and a connection portion (102), wherein the action portion (101) and the liner structure (2) are matched and combined, and the connection portion (102) is fixedly connected to a natural bone or an artificial bone; The action portion (101) and the connection portion (102) both include a base structure (11) arranged on the inner side, the action portion (101) also includes an intermediate layer (12) adhered to the outer side of the base structure (11) and a surface layer (13) adhered to the outer side of the intermediate layer (12); the connection portion (102) also includes a fusion layer (14) adhered to the outer side of the base structure (11).
2. The titanium alloy artificial bone joint with low friction coefficient according to claim 1, characterized in that: The matrix structure (11) comprises the following raw material components in proportion by weight: Titanium: ≥85%, Nitrogen: 5-10%, Aluminum: 2-8%, Vanadium: 1-2%.
3. The titanium alloy artificial bone joint with low friction coefficient according to claim 2, characterized in that: The matrix structure (11) further comprises the following raw material components in proportion by weight: Iron: ≤0.25%, Zirconium: ≤0.3%, Molybdenum: ≤1.5%.
4. The titanium alloy artificial bone joint with low friction coefficient according to claim 3, characterized in that: The fusion layer (14) comprises the following raw material components in proportion by weight: Titanium: 85-90%, Bioactive glass: 10-15%; The bioactive glass comprises the following raw material components in proportion by weight: Silicon dioxide: 45-52%, Calcium oxide: 25-30%, Sodium oxide: 10-15%, Phosphorus oxide: 2-6%.
5. The titanium alloy artificial bone joint with low friction coefficient according to claim 4, characterized in that: The middle layer (12) is evenly provided with anchor holes (121) on one side facing the liner structure (2), and the middle layer (12) comprises the following raw material components in proportion by weight: Titanium: 85-95%, Tantalum: 5-10%, Niobium: 1-5%, Ceramic matrix composite materials: ≤5%; The ceramic matrix composite material comprises the following raw material components in proportion by weight: Alumina: 70-80%, Zirconia: 20-30%, Additives: ≤5%; The additives include one or more of silicon dioxide, titanium oxide, and rare earth oxides.
6. The titanium alloy artificial bone joint with low friction coefficient according to claim 5, characterized in that: The surface layer (13) is a nitrogen-containing high-carbon nanocrystalline titanium alloy coating, and the nitrogen-containing high-carbon nanocrystalline titanium alloy coating comprises the following raw material components in proportion by weight: Nanocrystalline titanium: ≥80%, Nitrogen: 4-8%, Charcoal: 2-5%.
7. The titanium alloy artificial bone joint with low friction coefficient according to claim 6, characterized in that: The liner structure (2) comprises the following raw material components in proportion by weight: PEEK: 90-95%, Tetrafluoroethylene fiber: 5-10%.
8. A preparation method of a titanium alloy artificial bone joint with a low friction coefficient according to claim 7 is provided, characterized in that: The method comprises the following steps for preparing a joint component (1): S1-1. Preparation of the matrix structure (11): S1-1-1: preparing a blank by a melt casting method; S1-1-2: the surface of the blank is subjected to cutting and finishing, polishing of the edges and corners, sandblasting, and cleaning in sequence to obtain a base structure (11) having a connecting portion (102) and an action portion (101); S1-2. Preparation of Fusion Layer (14): S1-2-1: performing a coating treatment on the base structure (11) of the action part (101), installing a coating shell on the outside of the action part (101), and forming a fusion layer (14) on the outer surface of the base structure (11) of the connection part (102) by a vapor deposition method; S1-2-2: removing the outer covering shell of the action part (101), and cleaning the base structure (11) of the action part (101); S1-3. Preparation of the intermediate layer (12): S1-3-1: coating the fusion layer (14) of the connection part (102), installing a coating shell on the outside of the fusion layer (14), and forming an intermediate layer (12) on the outer surface of the base structure (11) of the action part (101) by a vapor deposition method; S1-3-2: drilling a hole on a side of the middle layer (12) facing the liner structure (2) to form the anchor hole (121), and using a spraying process to form a surface layer (13) on the outer surface of the middle layer (12), so that the surface layer (13) enters the anchor hole (121) to enhance the bonding stability between the surface layer (13) and the middle layer (12); S1-3-3: removing the outer covering shell of the fusion layer (14), and cleaning the entire joint component (1), thereby completing the preparation of the joint component (1); The method further comprises the following steps for preparing the liner structure (2): S2: A one-piece cushion structure (2) is produced by melt casting.
9. A preparation method according to claim 8, characterized in that: The coating shell is made of high temperature resistant material, and the coating treatment and removal of the coating shell include: S3-1: The covering shell is detachably mounted on the outside of the base structure (11) of the action part (101) or the outside of the fusion layer (14) of the connection part (102); S3-2: removing the outer covering shell of the base structure (11) of the action part (101) or the outer covering shell of the fusion layer (14) of the connection part (102).
Citation Information
Patent Citations
Mo metal doped composite diamond-like coating titanium alloy artificial bone joint and manufacturing method thereof
CN103920185A
Prosthesis component and method for manufacturing same
CN104840273A
Artificial joint material
CN107029284A
Medical device
CN113230462A
Artificial skeleton joint and preparation method thereof