A method for strengthening laser 3D printing of SiC blanks based on a dual binder system

Through the dual binder system and liquid silicon permeation technology, the strength and reliability problems of laser 3D printing of SiC blanks are solved, and high strength and high reliability manufacturing of large-size complex components are achieved.

CN118561599BActive Publication Date: 2024-12-03SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411045000.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-12-03
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The existing laser 3D printed SiC blank has high porosity and low strength after debonding, which limits the application of large-size complex components and is prone to cracks and fracture problems.

Method used

The combination of high-residual carbon organics and low-residual carbon organics is adopted to improve the strength after printing and debonding through different carbonization behaviors and thermal stress management, and achieve densification through liquid silicon penetration.

Benefits of technology

It significantly improves the strength and reliability of laser 3D printing SiC blanks, and is suitable for the manufacturing of large-size complex components, with a bending strength of 200~250 MPa.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118561599B_ABST
    Figure CN118561599B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for strengthening laser 3D printing of SiC blanks based on a dual binder system. The method comprises: (1) mixing SiC powder, a first binder and a second binder to obtain a composite powder; wherein, based on the total volume of the composite powder being 100 vol%, the volume proportion of SiC powder is 46-80 vol%, the volume proportion of the first binder is 5-29 vol%, and the volume proportion of the second binder is 1-25 vol%; the first binder is a high carbon residue organic matter; the carbon residue rate of the high carbon residue organic matter is 25-50%; the second binder is a low carbon residue organic matter; the carbon residue rate of the low carbon residue organic matter is 0.5-20%; (2) performing selective laser printing on the composite powder, and then performing a debonding treatment to obtain a laser 3D printed SiC blank. The method of the present invention provides a basis for the application of laser 3D printing of large-scale complex components.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of material preparation in additive manufacturing, and specifically relates to a method for strengthening laser 3D printing (also known as selective laser sintering, SLS) of SiC blanks based on a double binder system. Background Art

[0002] Additive manufacturing technology (or 3D printing technology) has developed significantly and rapidly in the past few decades and has received great attention. The principle of additive manufacturing technology is based on the principle of discrete material accumulation. It converts the three-dimensional digital model into a continuously superimposed two-dimensional thin film model, and then deposits the raw materials layer by layer under the control of a computer program to construct the component. Compared with traditional equal-material manufacturing and subtractive manufacturing technology, additive manufacturing technology is not limited by molds or processing technology, solves the problem of difficult structural forming of complex-shaped products, reduces processing procedures, shortens processing cycles, and greatly saves processing costs. Moreover, the more complex the product structure, the more obvious the advantages of additive manufacturing technology. Therefore, it is widely used in the manufacture of polymers, metals and some ceramic components. In particular, for the manufacture of high-hardness and high-brittle materials such as SiC, additive manufacturing has incomparable advantages. Among them, laser 3D printing (also known as Selective Laser Sintering, SLS) technology is one of the more mature technologies in additive manufacturing. Its working principle is: spread the raw material powder on the powder bed through a roller or scraper; use high-energy laser pulses to sinter the powder to combine it together, and then spread the powder and sinter it; repeat this process until the part is completed. SLS molding is fast and simple, and can achieve rapid near-net-shape manufacturing of complex structural parts.

[0003] However, the current SLS-printed SiC blanks have a high porosity, low strength and poor reliability after debonding, which has brought many adverse effects on SLS printing of large-scale SiC complex components (especially the handling and flipping of large-scale blanks). SLS printing is a powder-embedded printing method. When printing large-scale lightweight complex structural parts, if the sample is not strong enough when it is fished out of the powder, it is easy to crack or even break. When the large-scale components are placed, the bottom part will bear a large gravity. Therefore, the low-strength SiC blanks in the prior art limit the application of SLS printing in the preparation of large-scale complex components. Summary of the invention

[0004] In view of the above problems, the present invention provides a method for strengthening laser 3D printing of SiC blanks based on a dual binder system, comprising:

[0005] (1) SiC powder, a first binder and a second binder are mixed to obtain a composite powder; wherein, based on the total volume of the composite powder being 100 vol%, the volume proportion of the SiC powder is 46 to 80 vol%, the volume proportion of the first binder is 5 to 29 vol%, and the volume proportion of the second binder is 1 to 25 vol%; the first binder is a high-carbon residual organic matter; the carbon residual rate of the high-carbon residual organic matter is 25 to 50%; the second binder is a low-carbon residual organic matter; the carbon residual rate of the low-carbon residual organic matter is 0.5 to 20%;

[0006] (2) The composite powder is subjected to selective laser printing and then debonding treatment to obtain a laser 3D printed SiC blank.

[0007] The inventors found that since laser 3D printing is formed by laser heating to soften the adhesive, and the adhesive solidifies and connects the printed matrix powder, the performance of the printed blank is related to the type of adhesive and the connection state of the printing. For this reason, the inventors specifically use dual adhesives (high carbon residue organic matter and low carbon residue organic matter) to carry out selective laser printing of SiC ceramic composite materials, and use the different physical properties of adhesives with different carbon residue rates before and after 3D printing debonding to achieve strength improvement after printing and debonding. Since the C content of high carbon residue adhesives is relatively high and the corresponding carbon chain is longer and the functional groups are less, they often show different carbonization behavior from low carbon residue adhesives during the carbonization process, with a relatively wide carbonization temperature range and a long carbonization time. Low carbon residue adhesives have relatively low C content, short carbon chains, and more functional groups. The temperature range during carbonization is narrow, and they are rapidly carbonized in a very short range. The rapid carbonization of low carbon residue binder will bring greater thermal stress to the sample (low carbon residue binder carbonization process is very fast, under the same system, low carbon residue binder will lose more mass, the corresponding volume change will also be greater, which causes greater thermal stress), and due to its own low carbon residue characteristics, it will cause the performance of the sample blank to decline; high carbon residue binder has a wide carbonization temperature range and a mild carbonization process, but its high melting point leads to its relatively poor connectivity during printing, which will also cause the performance of the sample blank to decline. The use of high carbon residue binder and low carbon residue binder for selective laser printing of SiC ceramic composites can not only improve the connectivity during printing, but also avoid the sample from generating high stress during carbonization, and improve the reliability of the printed blank. Liquid silicon infiltration (LSI) is used to remove carbon residue, and the carbon residue reacts with molten Si to form SiC to achieve densification. At the same time, the inventors also found that the introduction of low carbon residue binder will affect the fluidity of the composite powder. Compared with the high carbon residue binder, the low carbon residue binder has more groups, which will cause it to carry more static charge during ball milling. Improving the fluidity of the composite powder is helpful for printing and molding.

[0008] The method for strengthening the laser 3D printing SiC blank based on the dual binder system provided by the present invention can improve the strength of the laser 3D printed blank of the silicon carbide ceramic composite material and its strength after debonding, improve its reliability, and provide a basis for the application of laser 3D printing of large-scale complex components.

[0009] Preferably, in step (1), the particle size of the SiC powder is 5 to 80 μm; the density of the SiC powder is 3.0 to 3.2 g / cm 3 .

[0010] Preferably, in step (1), the high carbon residue organic matter is at least one of phenolic resin (PR), asphalt resin, and urea-formaldehyde resin; the density of the high carbon residue organic matter is 1.0-1.5 g / cm 3 .

[0011] Preferably, in step (1), the low carbon residue organic matter is at least one of epoxy resin (EP), polyamide (PA), PVA, PMMA, and PVB; the density of the low carbon residue organic matter is 0.5 to 1.2 g / cm 3 ; The low residual carbon organic matter accounts for 1 / 30 to 5 / 6 of the total volume content of the high residual carbon organic matter and the low residual carbon organic matter.

[0012] Preferably, in step (1), the mixing method is ball milling; the parameters of the ball milling mixing include: ball milling speed of 60 to 600 r / min, ball milling time of 2 to 12 h, and ball-to-material ratio of (2 to 5): 1;

[0013] After ball milling and mixing, the mixture is sieved; the mesh number of the sieve is 50 to 300 meshes.

[0014] Preferably, in step (2), the parameters of the selected area laser printing include: laser power of 30 to 60 W; scanning speed of 100 to 7620 mm / s; layer thickness of 0.05 to 0.2 mm; and scanning spacing of 0.08 to 0.3 mm.

[0015] Preferably, in step (2), the parameters of the debonding treatment include: the atmosphere is a vacuum atmosphere, an argon atmosphere or a nitrogen atmosphere; the temperature of the debonding treatment is 600 to 1200° C.; and the time of the debonding treatment is 30 to 90 min.

[0016] Furthermore, preferably, the parameters of the debonding treatment include: in a vacuum, argon or nitrogen atmosphere, heating to 150-300 ° C at a heating rate of 1-3 ° C / min, then continuing to heat to 200-600 ° C at a heating rate of 0.25-2 ° C / min, and finally heating to 600-1200 ° C at a heating rate of 1-3 ° C / min and keeping warm for 30-90 min, and then cooling to room temperature.

[0017] In a second aspect, the present invention provides a laser 3D printed SiC blank prepared according to the above method, wherein the strength of the laser 3D printed SiC blank is at least 2.5 MPa.

[0018] In a third aspect, the present invention provides a method for preparing a laser 3D printed silicon carbide ceramic composite material, comprising: subjecting the laser 3D printed SiC blank to siliconization treatment to obtain a laser 3D printed silicon carbide ceramic composite material.

[0019] Preferably, the parameters of the siliconizing treatment include: the atmosphere is vacuum, argon atmosphere or nitrogen atmosphere; the temperature of the siliconizing treatment is 1450-1700° C.; and the time of the siliconizing treatment is 30-120 min.

[0020] Furthermore, preferably, the parameters of the siliconizing treatment include: in a vacuum, argon or nitrogen atmosphere, heating to 1000-1200°C at a heating rate of 5-10°C / min, then continuing to heat to 1200-1400°C at a heating rate of 3-5°C / min, finally heating to 1450-1700°C at a heating rate of 1-3°C / min and keeping warm for 30-120min, then cooling to 1000-1350°C at a cooling rate of 1-2.5°C / min, and finally cooling to room temperature.

[0021] In a fourth aspect, the present invention provides a laser 3D printed silicon carbide ceramic composite material prepared according to the above preparation method, wherein the laser 3D printed silicon carbide ceramic composite material has a flexural strength of 200 to 250 MPa.

[0022] In the present invention, a dual binder is used to print silicon carbide ceramic composite materials. The green blank printed by the dual binder has high strength and better reliability, which is more conducive to the application of laser 3D printing in the preparation of large and complex components. The laser 3D printed SiC green blank prepared by the present invention has high strength and good reliability, providing a basis for the application of laser 3D printing of large-scale complex components.

[0023] Beneficial effects of the present invention:

[0024] Compared with the prior art, the present invention mainly has the following technical advantages:

[0025] (1) Based on the effect of the dual binder, the present invention enables the laser 3D printed samples to maintain excellent strength both after printing and after debonding;

[0026] (2) The low residual carbon binder in the dual binder of the present invention acts as a pore former after debonding, which is beneficial to improving the uniformity of siliconization and the strength of the siliconized sample;

[0027] (3) In order to solve the problem that organic binders will be charged with static electricity due to friction during ball milling, thus causing uneven mixing, the present invention uses dual binders with different functional groups having different electron gain and loss abilities, resulting in more uniform sample mixing;

[0028] (4) In the present invention, since the low carbon residue binder itself has more functional groups, it will carry more static charge during ball milling, thereby improving the fluidity of the composite powder. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 (a)-(i) are SEM images of the SiC blanks printed without debonding treatment in Comparative Example 1, Examples 7-8, Examples 1-5 and Comparative Example 2, respectively;

[0030] Figure 2 (a)-(i) are SEM images of the SiC blanks after debonding in Comparative Example 1, Examples 7-8, Examples 1-5 and Comparative Example 2, respectively;

[0031] Figure 3 This is a SEM image of the SiC blank after debonding in Comparative Example 3;

[0032] Figure 4 (a)-(c) are SEM images of the silicon carbide ceramic composite materials in Comparative Example 1, Example 6 and Comparative Example 2, respectively;

[0033] Figure 5 Thermogravimetric analysis of phenolic resin (PR);

[0034] Figure 6 Thermogravimetric analysis of epoxy resin (EP);

[0035] Figure 7 The Carr index and the Hausenner ratio of the composite powders of Examples 1-5, Examples 7-8 and Comparative Examples 1-3;

[0036] Figure 8 Infrared spectra of phenolic resin (PR), epoxy resin (EP) and polyamide (PA). DETAILED DESCRIPTION

[0037] To further explain the content, characteristics and practical effects of the present invention, the present invention is described in detail below in conjunction with the embodiments. It should be pointed out that the modification method of the design of the present invention is not limited to these specific embodiments. Without departing from the spirit and connotation of the design of the present invention, the equivalent replacement and modification made by those skilled in the art on the basis of reading the content of the present invention are also within the scope of the present invention. In the absence of special instructions, each percentage refers to the volume percentage.

[0038] In the present invention, a dual binder is used for selective laser printing of SiC ceramic composite materials, and the different physical properties of binders with different residual carbon rates before and after 3D printing debonding are used to achieve strength improvement after printing and after debonding. Specifically, low residual carbon binders generally have a relatively lower melting point, and the rich functional groups make their wettability with SiC better, so that the SiC blank has higher strength after printing, but the low residual carbon rate leads to a decrease in the pyrolytic carbon content that plays a connecting role in the debonded blank, and the strength after debonding is low. The high residual carbon binder mainly utilizes its high residual carbon characteristics to provide more pyrolytic carbon while participating in the connection. Therefore, when they are used in combination, the synergistic effect between the two leads to an improvement in the final performance.

[0039] The following is an exemplary description of the method for strengthening laser 3D printing of SiC blanks based on a dual binder system provided by the present invention.

[0040] Preparation of composite powder for laser 3D printing. SiC powder, high residual carbon organic matter as the first binder and low residual carbon organic matter as the second binder are ball-milled and sieved to obtain composite powder for laser 3D printing. Wherein, based on the total volume of the composite powder for laser 3D printing being 100 vol%, the volume proportion of SiC powder is 46-80 vol%, the volume proportion of the first binder is 5-29 vol%, and the volume proportion of the second binder is 1-25 vol%. If the content of the first binder is too much, the connection between the binder and SiC is insufficient, resulting in insufficient strength of the printed blank; if the content of the second binder is too much, the content of pyrolytic carbon that plays a connecting role in the debonded blank is reduced, resulting in insufficient strength of the debonded blank. The Carr index of the composite powder for laser 3D printing can be 0.14-0.25, and the Hausner ratio can be 1.16-1.34.

[0041] In an optional embodiment, the particle size of the SiC powder is 5 to 80 μm. The density of the SiC powder is 3.0 to 3.2 g / cm 3 For example, the density is 3.20 g / cm 3 The low carbon residue organic matter accounts for 1 / 30 to 5 / 6 (for example, 1 / 30, 1 / 10, 1 / 6, 1 / 3, 1 / 2, 2 / 3, 4 / 5, 5 / 6, etc.) of the total volume content of the high carbon residue organic matter and the low carbon residue organic matter.

[0042] In an optional embodiment, the first binder is a high carbon residue organic matter. The high carbon residue organic matter may be at least one of phenolic resin, asphalt resin, urea-formaldehyde resin, etc. The density of the high carbon residue organic matter is 1.0-1.5 g / cm 3 , for example 1.10 g / cm 3The second binder is a low carbon residue organic matter. The low carbon residue organic matter may be at least one of epoxy resin, polyamide, polyvinyl alcohol PVA, polymethyl methacrylate PMMA, polyvinyl butyral PVB, etc. The density of the low carbon residue organic matter is 0.5-1.2 g / cm 3 , for example 1.10 g / cm 3 As an example of preparing a composite powder, the process includes ball milling and sieving SiC powder, epoxy resin (EP) and phenolic resin (PR) to obtain a composite powder for laser printing.

[0043] In an optional embodiment, the parameters of the ball milling include: the ball milling speed may be 60-600 r / min, the ball milling time may be 2-12 h, and the ball milling material ratio may be (2-5): 1. The mesh size of the sieving may be 50-300 meshes.

[0044] Preparation of porous SiC blank: The composite powder for laser 3D printing is subjected to selective laser printing to obtain a laser 3D printed porous SiC blank (or printed body).

[0045] In an optional embodiment, the parameters of the selective laser printing include: the laser power may be 30 to 60 W; the scanning speed may be 100 to 7620 mm / s; the layer thickness may be 0.05 to 0.2 mm, for example, 0.1 mm; and the scanning interval may be 0.08 to 0.3 mm.

[0046] Debonding treatment: The obtained laser 3D printed porous SiC blank is subjected to debonding treatment to obtain a 3D printed SiC blank (or debonded body).

[0047] In an optional embodiment, the parameters of the debonding treatment include: in a vacuum, argon or nitrogen atmosphere, heating the printed body to 600-1200°C and keeping it at this temperature for 30-90 minutes. For example, heating to 150-300°C at a heating rate of 1-3°C / min, then continuing to heat to 200-600°C at a heating rate of 0.25-2°C / min, and finally heating to 600-1200°C at a heating rate of 1-3°C / min and keeping it at this temperature for 30-90 minutes, and then cooling to room temperature. As an example, the porous SiC blank is debonded for 30 minutes under vacuum and 900°C.

[0048] The following is an exemplary description of a method for preparing a laser 3D printed silicon carbide ceramic composite material.

[0049] Siliconizing treatment: The laser 3D printed porous SiC blank after debonding treatment is siliconized to obtain a laser 3D printed silicon carbide ceramic composite material.

[0050] In an optional embodiment, the parameters of the siliconizing treatment include: heating the laser 3D printed porous SiC blank after debonding to 1450-1700 ° C and keeping it warm for 30-120 min in a vacuum, argon or nitrogen atmosphere. For example, heating to 1000-1200 ° C at a heating rate of 5-10 ° C / min, and then continuing to heat to 1200-1400 ° C at a heating rate of 3-5 ° C / min, and finally heating to 1450-1700 ° C at a heating rate of 1-3 ° C / min and keeping it warm for 30-120 min, then cooling by 1000-1350 at a cooling rate of 1-2.5 ° C / min, and finally cooling to room temperature. As an example, the laser 3D printed porous SiC blank after debonding is siliconized for 30 min at 1550 ° C in a vacuum.

[0051] In the present invention, the flexural strength of the porous SiC blank after laser 3D printing is tested by a three-point bending test (Instron-1195, Instron, USA) to be 2.56-4.49 MPa. The flexural strength of the porous SiC blank after debonding treatment is tested by a three-point bending test (Instron-1195, Instron, USA) to be 4.31-6.82 MPa. The flexural strength of the silicon carbide ceramic composite material after siliconization is tested by a three-point bending test (Instron-1195, Instron, USA) to be 200-250 MPa.

[0052] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make selections within a suitable range through the description of this article, and are not limited to the specific values ​​​​exemplified below. The percentage content in the following examples and comparative examples is calculated by volume percentage.

[0053] Example 1 (70 vol% SiC-5 vol% EP-25 vol% PR)

[0054] (1) 70 vol% SiC, 5 vol% EP and 25 vol% PR powders were ball milled at a ball milling speed of 60 r / min, a ball-to-material ratio of 2:1 and a ball milling time of 2 h; after ball milling, the powders were sieved through a 200 μm sieve to obtain composite powders for laser 3D printing;

[0055] (2) performing selective laser printing on the obtained composite powder for laser 3D printing to obtain a laser 3D printed porous SiC blank; wherein the selective laser printing parameters include: laser power of 45 W, scanning speed of 7620 mm / s, layer thickness of 0.1 mm, and scanning spacing of 0.08 mm;

[0056] (3) The obtained laser 3D printed porous SiC blank was debonded under vacuum and 900 °C for 30 min to obtain a debonded laser 3D printed porous SiC blank; wherein the temperature was increased to 200 °C at a heating rate of 3 °C / min, then continued to be increased to 600 °C at a heating rate of 2 °C / min, and finally increased to 900 °C at a heating rate of 3 °C / min and kept at this temperature for 30 min, and then cooled to room temperature.

[0057] In this Example 1, the flexural strength of the porous SiC blank after laser 3D printing is 3.3019 MPa, and the flexural strength of the porous SiC blank after debonding is 6.8213 MPa.

[0058] Example 2 (70 vol% SiC-10 vol% EP-20 vol% PR)

[0059] The preparation process of the laser 3D printing porous SiC blank after debonding in this embodiment 2 refers to that in embodiment 1, except that in step (1), the composition of the composite powder for laser 3D printing is: 70 vol% SiC, 10 vol% EP and 20 vol% PR. The other steps are the same as in embodiment 1.

[0060] In this Example 2, the flexural strength of the porous SiC blank after laser 3D printing is 3.4721 MPa, and the flexural strength of the porous SiC blank after debonding is 6.1875 MPa.

[0061] Example 3

[0062] The preparation process of the laser 3D printing porous SiC blank after debonding in this embodiment 3 refers to that in embodiment 1, except that in step (1), the composition of the composite powder for laser 3D printing is: 70 vol% SiC, 15 vol% EP and 15 vol% PR. The other steps are the same as in embodiment 1.

[0063] In this Example 3, the flexural strength of the porous SiC blank after laser 3D printing is 3.6068 MPa, and the flexural strength of the porous SiC blank is 5.1726 MPa.

[0064] Example 4 (70 vol% SiC-20 vol% EP-10 vol% PR)

[0065] The preparation process of the laser 3D printing porous SiC blank after debonding in this embodiment 4 is similar to that in embodiment 1, except that in step (1), the composition of the composite powder for laser 3D printing is 70 vol% SiC, 20 vol% EP and 10 vol% PR. The other steps are the same as those in embodiment 1.

[0066] In this Example 4, the flexural strength of the porous SiC blank after laser 3D printing is 4.4929 MPa, and the flexural strength of the porous SiC blank is 5.2324 MPa.

[0067] Example 5 (70 vol% SiC-25 vol% EP-5 vol% PR)

[0068] The preparation process of the laser 3D printing porous SiC blank after debonding in this embodiment 5 refers to that in embodiment 1, except that in step (1), the composition of the composite powder for laser 3D printing is: 70 vol% SiC, 25 vol% EP and 5 vol% PR. The other steps are the same as in embodiment 1.

[0069] In this Example 5, the flexural strength of the porous SiC blank after laser 3D printing is 3.6845 MPa, and the flexural strength of the porous SiC blank is 4.3126 MPa.

[0070] Example 6

[0071] The debonded laser 3D printed porous SiC blank prepared in Example 2 was siliconized for 30 min at 1550° C. under vacuum conditions to obtain a laser 3D printed SiC ceramic composite material.

[0072] The strength of the laser 3D printed SiC ceramic composite material obtained in this Example 6 is 239.6785 MPa.

[0073] Example 7 (70 vol% SiC-1 vol% EP-29 vol% PR)

[0074] The preparation process of the laser 3D printing porous SiC blank after debonding in this embodiment 7 refers to that in embodiment 1, except that in step (1), the composition of the composite powder for laser 3D printing is: 70 vol% SiC, 1 vol% EP and 29 vol% PR. The other steps are the same as in embodiment 1.

[0075] In this Example 7, the flexural strength of the porous SiC blank after laser 3D printing is 2.5635 MPa, and the flexural strength of the porous SiC blank is 4.4873 MPa.

[0076] Example 8 (70 vol% SiC-3 vol% EP-27 vol% PR)

[0077] The preparation process of the laser 3D printing porous SiC blank after debonding in this Example 8 is similar to that in Example 1, except that in step (1), the composition of the composite powder for laser 3D printing is 70 vol% SiC, 3 vol% EP and 27 vol% PR. The other steps are the same as those in Example 1.

[0078] In this Example 8, the flexural strength of the porous SiC blank after laser 3D printing is 2.9157 MPa, and the flexural strength of the porous SiC blank is 5.0639 MPa.

[0079] Comparative Example 1 (70 vol% SiC-0 vol% EP-30 vol% PR)

[0080] The preparation process of the laser 3D printed porous SiC blank after debonding in this comparative example 1 refers to Example 1, except that in step (1), the composition of the composite powder for laser 3D printing is: 70 vol% SiC, 0 vol% EP and 30 vol% PR. The other steps are the same as in Example 1. The preparation process of the laser 3D printed SiC ceramic composite material in this comparative example 1 refers to Example 6.

[0081] In this comparative example 1, the flexural strength of the porous SiC blank after laser 3D printing is 2.0165 MPa, and the flexural strength of the porous SiC blank is 4.1500 MPa. The flexural strength of the obtained silicon carbide ceramic composite material after siliconization is 196.1043 MPa.

[0082] Comparative Example 2 (70 vol% SiC-30 vol% EP-0 vol% PR)

[0083] The preparation process of the laser 3D printed porous SiC blank after debonding in this comparative example 2 refers to Example 1, except that in step (1), the composition of the composite powder for laser 3D printing is: 70 vol% SiC, 30 vol% EP and 0 vol% PR. The other steps are the same as in Example 1. The preparation process of the laser 3D printed SiC ceramic composite material in this comparative example 2 refers to Example 6.

[0084] In this comparative example 2, the flexural strength of the porous SiC blank after laser 3D printing is 4.5249 MPa, and the flexural strength of the porous SiC blank is 1.0141 MPa. The flexural strength of the obtained silicon carbide ceramic composite material after siliconization is 216.6727 MPa.

[0085] Comparative Example 3 (70 vol% SiC-10 vol% EP-15 vol% PR-5% MCMB (spherical graphite))

[0086] The preparation process of the laser 3D printing porous SiC blank after debonding in this comparative example 3 refers to that in Example 1, except that in step (1), the composition of the composite powder for laser 3D printing is: 70 vol% SiC, 10 vol% EP, 15 vol% PR and 5% MCMB. The other steps are the same as in Example 2.

[0087] In this comparative example 3, the flexural strength of the porous SiC blank after laser 3D printing is 3.3616 MPa, and the flexural strength of the porous SiC blank is 4.7888 MPa.

[0088] Table 1 lists the performance parameters of the porous SiC blanks after laser 3D printing and the porous SiC blanks after debonding in Examples 1-5, Examples 7-8 and Comparative Examples 1-3 of the present invention.

[0089] Table 1:

[0090] .

[0091] As can be seen from Table 1, the dual adhesive is even inferior to the pure low carbon residue adhesive in improving the mechanical properties of the printed body of the sample, but the dual adhesive has a significant advantage in improving the mechanical properties of the debonded body of the sample.

[0092] Figure 1 (a)-(i) are SEM images of the printed blanks of Comparative Example 1, Examples 7-8, Examples 1-5 and Comparative Example 2. The higher the content of EP, the better the connectivity between SiC particles.

[0093] Figure 2 (a)-(i) are SEM images of the debonded green blanks of Comparative Example 1, Examples 7-8, Examples 1-5 and Comparative Example 2. The low carbon residue rate of EP leads to a decrease in the connectivity of high EP content.

[0094] Figure 3 This is a SEM picture of the SiC blank after debonding in comparative example 3. It can be seen from the figure that the spherical graphite does not melt and participate in the connection.

[0095] Figure 4 (a) to (c) are SEM images of the silicon carbide ceramic composite materials of Comparative Example 1, Example 6 and Comparative Example 2. As can be seen from the figure, the SiC ceramics prepared by the method of the present invention have a uniform microstructure.

[0096] Figure 5-6 Thermogravimetric analysis of phenolic resin (PR) and epoxy resin (EP) are shown in Figure 1. As can be seen from the figure, the thermophysical properties of the two resins are quite different, which meets the experimental requirements of the present invention.

[0097] Figure 7The Carr index and Hausenner ratio are the composite powders of Examples 1-5, Examples 7-8 and Comparative Examples 1-3 (the two are different evaluation criteria for characterizing the fluidity of powders, and the smaller the value, the better the fluidity). It can be seen from the figure that the low carbon residue binder combined with the high carbon residue binder system can effectively improve the fluidity of the composite powder.

[0098] Figure 8 The infrared spectra of phenolic resin (PR), epoxy resin (EP) and polyamide (PA) are shown in Figure 1. As shown in the figure, low binders (EP, PA) have more functional groups than high carbon residue binders (PR), which helps to improve the fluidity of the composite powder.

[0099] Refer to Comparative Example 1, only high residual carbon binder is used, and due to its physical properties, its strength and toughness after printing are insufficient. Refer to Comparative Example 2, only low residual carbon binder is used, although it has good strength after printing, but due to the characteristics of low residual carbon, the strength after debonding is often very low. Refer to Comparative Example 3, the method of using inorganic carbon (such as carbon black, graphite, etc.) to replace organic binder for printing cannot effectively improve the performance of the sample blank. The organic carbon source will soften and bond during the printing process to connect the printed matrix powder such as SiC, while the inorganic carbon will not soften and bond during the printing process, so its effect on the performance of the sample blank is minimal compared to the binder.

Claims

1. A method for strengthening laser 3D printing of SiC blanks based on a dual binder system, characterized in that: include: (1) SiC powder, a first binder and a second binder are mixed to obtain a composite powder; wherein, based on the total volume of the composite powder being 100 vol%, the volume proportion of the SiC powder is 46 to 80 vol%, the volume proportion of the first binder is 5 to 29 vol%, and the volume proportion of the second binder is 1 to 25 vol%; the first binder is a high carbon residue organic matter; the carbon residue rate of the high carbon residue organic matter is 25 to 50%; the high carbon residue organic matter is at least one of phenolic resin, asphalt resin and urea-formaldehyde resin; the density of the high carbon residue organic matter is 1.0 to 1.5 g / cm 3 ; The second binder is a low carbon residue organic matter; the carbon residue rate of the low carbon residue organic matter is 0.5-20%; the low carbon residue organic matter is at least one of epoxy resin, polyamide, PVA, PMMA, and PVB; the density of the low carbon residue organic matter is 0.5-1.2 g / cm 3 ; The low residual carbon organic matter accounts for 1 / 6 to 2 / 3 of the total volume content of the high residual carbon organic matter and the low residual carbon organic matter; (2) The composite powder is subjected to selective laser printing and then subjected to a debonding treatment to obtain a laser 3D printed SiC blank; the parameters of the debonding treatment include: heating to 150-300°C at a heating rate of 1-3°C / min under a vacuum, argon or nitrogen atmosphere, then further heating to 200-600°C at a heating rate of 0.25-2°C / min, and finally heating to 600-1200°C at a heating rate of 1-3°C / min and keeping the temperature for 30-90 min, and then cooling to room temperature.

2. The method according to claim 1, characterized in that In step (1), the particle size of the SiC powder is 5 to 80 μm; the density of the SiC powder is 3.0 to 3.2 g / cm 3 .

3. The method according to any one of claims 1 to 2, characterized in that In step (1), the mixing method is ball milling; the parameters of the ball milling mixing include: a ball milling speed of 60 to 600 r / min, a ball milling time of 2 to 12 h, and a ball-to-material ratio of (2 to 5): 1; After ball milling and mixing, the mixture is sieved; the mesh number of the sieve is 50 to 300 meshes.

4. The method according to any one of claims 1 to 2, characterized in that In step (2), the parameters of the selected area laser printing include: laser power of 30 to 60 W; scanning speed of 100 to 7620 mm / s; layer thickness of 0.05 to 0.2 mm; and scanning spacing of 0.08 to 0.3 mm.

5. A laser 3D printed SiC blank prepared according to the method of claim 1, characterized in that: The strength of the laser 3D printed SiC blank is at least 2.5 MPa.

6. A method for preparing a laser 3D printed silicon carbide ceramic composite material, characterized in that: include: The laser 3D printed SiC blank according to claim 5 is subjected to siliconization treatment to obtain a laser 3D printed silicon carbide ceramic composite material.

7. The preparation method according to claim 6, characterized in that The parameters of the siliconizing treatment include: the atmosphere is vacuum, argon atmosphere or nitrogen atmosphere; the temperature of the siliconizing treatment is 1450-1700° C.; and the time of the siliconizing treatment is 30-120 minutes.

8. The preparation method according to claim 7, characterized in that The parameters of the siliconizing treatment include: in a vacuum, argon or nitrogen atmosphere, heating to 1000-1200°C at a heating rate of 5-10°C / min, then continuing to heat to 1200-1400°C at a heating rate of 3-5°C / min, finally heating to 1450-1700°C at a heating rate of 1-3°C / min and keeping warm for 30-120 min, then cooling to 1000-1350°C at a cooling rate of 1-2.5°C / min, and finally cooling to room temperature.

9. A laser 3D printed silicon carbide ceramic composite material prepared by the preparation method according to any one of claims 6 to 8, characterized in that: The flexural strength of the laser 3D printed silicon carbide ceramic composite material is 200-250 MPa.

Citation Information

Patent Citations

  • Preparation method of laser 3D-printed complex-configuration silicon carbide composite part

    CN112624777A

  • Silicon carbide composite powder for additive manufacturing and preparation method thereof

    CN114230346A

  • Method for preparing silicon carbide composite material part through laser 3D printing based on grain composition composite technology

    CN115286408A

  • MCMB-based laser 3D printing Cf / SiC composite material and preparation method thereof

    CN118344167A