A method for preparing antistatic modified PVDF composite film
By using sodium bissulfonate-containing carbon nanotubes in PVDF and performing specific chemical treatment and casting film formation processes, the problem of PVDF materials being easy to trap charges and high agglomeration of carbon nanotubes is solved, and its anti-static properties are significantly improved and mechanical properties.
Patent Information
- Application Number
- CN202410617875.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-05-17
AI Technical Summary
PVDF materials are prone to trap charges, leading to insulation breakdown, short circuit and discharge phenomena, and carbon nanotubes are prone to agglomeration in PVDF, affecting the improvement of their antistatic properties.
Using a combination of sodium bissulfonate-containing carbon nanotubes and PVDF, the agglomeration of carbon nanotubes is reduced and a uniform conductive network is formed through specific chemical treatment and casting film formation processes, which enhances its compatibility in PVDF and Conductive properties.
The antistatic properties of PVDF composite films are significantly improved, and the combined effect of uniformly dispersing the carbon nanotubes and sodium bissulfonate structures effectively eliminates the electrostatic charge, improving the mechanical properties and antistatic properties of the material.
Smart Images

Figure CN118562163B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PVDF, in particular to a method for preparing an antistatic modified PVDF composite film. Background Art
[0002] Fluororesin has excellent electrical properties, mechanical properties, high temperature resistance and other properties, and is widely used in aerospace, insulation materials and other fields. PVDF is a typical fluororesin with excellent anti-oxidation and anti-ultraviolet properties, and is widely used in industrial materials. However, due to the high polarity of fluorine-carbon bonds, PVDF easily captures charges and forms space charges, which can cause insulation breakdown in severe cases, and eventually lead to insulation failure, short circuits, discharges and other phenomena, causing device failure. Therefore, how to inhibit the formation of PVDF charges, improve the charge distribution in PVDF, and enhance the antistatic properties of PVDF is one of the current research hotspots.
[0003] A common antistatic method is to add conductive materials such as copper, iron, silver, etc. to the material. Carbon nanotubes have excellent conductivity, so adding them to PVDF can also increase the antistatic performance of PVDF. However, carbon nanotubes are easy to entangle and have high surface activation energy, so they are easy to agglomerate in PVDF, which is not conducive to the improvement of PVDF's antistatic performance. Therefore, how to improve the agglomeration degree of carbon nanotubes in PVDF to improve its antistatic performance is one of the research hotspots. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides a method for preparing an antistatic modified PVDF composite film. The PVDF composite film prepared by the present invention has excellent antistatic properties.
[0006] (II) Technical solution
[0007] A method for preparing an antistatic modified PVDF composite film, the preparation method is as follows:
[0008] Disperse the carbon nanotubes containing sodium disulfonate in N,N-dimethylformamide solvent, add PVDF, stir and mix for 2-5 hours, let stand to degas, cast into a film on a horizontal glass plate, and dry in an oven at 70-85°C to obtain an antistatic modified PVDF composite film.
[0009] Preferably, the usage ratio of the sodium bissulfonate-containing carbon nanotubes and PVDF is (0.5-10) g:100 g.
[0010] Preferably, the preparation method of the carbon nanotubes containing sodium bissulfonate is:
[0011] (1) Add diaminobenzonitrile to acetonitrile solvent, stir and disperse, then add 1,3-propane sultone, heat to 80-100° C., react for 12-24 hours, cool to room temperature after the reaction, filter, wash with acetone, dry, then add to deionized water, stir and disperse, add sodium carbonate, react at 20-35° C. for 10-18 hours, dry to obtain intermediate 1.
[0012] (2) Under nitrogen conditions, intermediate 1 is added to a methanol solvent, stirred and dispersed, and then 5-10% palladium carbon and 30-40% hydrochloric acid are added thereto, and stirred for reaction. After the reaction is completed, the reaction is filtered, and the filtrate is distilled under reduced pressure and dried to obtain intermediate 2.
[0013] (3) Adding the acidified carbon nanotubes and thionyl chloride to N,N-dimethylformamide solvent, stirring and dispersing, heating to 100-110° C., reflux reaction for 15-30 hours, and after the reaction is completed, cooling to room temperature, and filtering under reduced pressure to obtain acyl chloride carbon nanotubes.
[0014] (4) dispersing the acyl chloride carbon nanotubes in N,N-dimethylformamide solvent, adding intermediate 2 thereto, stirring and dispersing, heating to 100-110° C., reflux reaction for 60-80 hours, filtering after the reaction, washing with deionized water, and drying to obtain carbon nanotubes containing sodium disulfonate.
[0015] Preferably, in step (1), the usage ratio of diaminobenzonitrile, 1,3-propane sultone and sodium carbonate is 1 g:(2-2.4) g:(1.5-2) g.
[0016] Preferably, in step (2), the stirring reaction time is 35-50 hours and the temperature is 20-35°C.
[0017] Preferably, in step (3), the usage ratio of the acidified carbon nanotubes to the dichlorothionyl is 1 g:(80-120) mL.
[0018] Preferably, in step (4), the usage ratio of acyl chloride carbon nanotubes to intermediate 2 is 1 g:(5-12) g.
[0019] (III) Beneficial technical effects
[0020] The present invention uses diaminobenzonitrile, 1,3-propane sultone, palladium carbon and the like as raw materials, undergoes ring-opening alkylation reaction and reduction reaction to obtain intermediate 2, which is then reacted with acyl chloride carbon nanotubes to prepare carbon nanotubes containing sodium bissulfonate. The carbon nanotubes containing sodium bissulfonate are added to PVDF, and cast into a film to obtain an antistatic modified PVDF composite film.
[0021] The carbon nanotubes used in the present invention have a nanometer size effect, so they are easy to agglomerate. The present invention makes them organic, reduces the agglomeration degree of the carbon nanotubes, increases their compatibility with organic substances, and adds them to PVDF, so that they can be evenly dispersed in PVDF to form a uniform conductive network, which can better play its antistatic effect. In addition, the modified PVDF composite film prepared by the present invention also contains a sodium disulfonate structure, and the ions generated after ionization can be used as a conductive medium to eliminate static charges in the material. It works together with the carbon nanotubes to promote the improvement of the antistatic performance of PVDF. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The invention is a preparation route of carbon nanotubes containing sodium disulfonate. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Preparation method of acidified carbon nanotubes: 0.5 g of multi-walled carbon nanotubes were added to 50 mL of concentrated nitric acid, ultrasonicated for 15 min, refluxed at 85° C. for 24 h, washed with deionized water, and dried to obtain acidified carbon nanotubes.
[0025] Example 1
[0026] (1) Add 2 g of diaminobenzonitrile to acetonitrile solvent, stir and disperse, then add 4.8 g of 1,3-propane sultone, heat to 90° C., react for 24 h, and after the reaction is completed, cool to room temperature, filter, wash with acetone, and dry. Then add it to deionized water, stir and disperse, add 3 g of sodium carbonate, react at 20° C. for 12 h, and after the reaction is completed, dry to obtain intermediate 1.
[0027] (2) Under nitrogen conditions, intermediate 1 was added to methanol solvent, stirred and dispersed, and then 6% palladium carbon and 35% hydrochloric acid were added thereto. The reaction was stirred at 30°C for 50 hours. After the reaction was completed, the reaction was filtered, and the filtrate was distilled under reduced pressure and dried to obtain intermediate 2.
[0028] (3) Add 1 g of acidified carbon nanotubes and 90 mL of dichlorothionyl into N,N-dimethylformamide solvent, stir and disperse, heat to 105° C., reflux for 20 h, and after the reaction is completed, cool to room temperature, and filter under reduced pressure to obtain chlorinated carbon nanotubes.
[0029] (4) Disperse 1 g of acyl chloride carbon nanotubes in N,N-dimethylformamide solvent, add 5 g of intermediate 2 thereto, stir and disperse, heat to 110° C., reflux for 70 h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain sodium disulfonate-containing carbon nanotubes.
[0030] (5) Disperse 0.1 g of carbon nanotubes containing sodium bissulfonate in N,N-dimethylformamide solvent, add 20 g of PVDF, stir and mix for 5 h, let stand to degas, cast on a horizontal glass plate, and dry in an oven at 80° C. to obtain an antistatic modified PVDF composite film.
[0031] Example 2
[0032] (1) Add 2 g of diaminobenzonitrile to acetonitrile solvent, stir and disperse, then add 4 g of 1,3-propane sultone, heat to 100° C., react for 12 h, and after the reaction is completed, cool to room temperature, filter, wash with acetone, and dry. Then add it to deionized water, stir and disperse, add 3 g of sodium carbonate, react at 35° C. for 18 h, and after the reaction is completed, dry to obtain intermediate 1.
[0033] (2) Under nitrogen conditions, intermediate 1 was added to methanol solvent, stirred and dispersed, and then 10% palladium carbon and 38% hydrochloric acid were added thereto. The reaction was stirred at 25°C for 40 hours. After the reaction was completed, the reaction was filtered, and the filtrate was distilled under reduced pressure and dried to obtain intermediate 2.
[0034] (3) Add 1 g of acidified carbon nanotubes and 120 mL of dichlorothionyl into N,N-dimethylformamide solvent, stir and disperse, heat to 110° C., reflux for 20 h, and after the reaction is completed, cool to room temperature, and filter under reduced pressure to obtain chlorinated carbon nanotubes.
[0035] (4) Disperse 1 g of acyl chloride carbon nanotubes in N,N-dimethylformamide solvent, add 12 g of intermediate 2 thereto, stir and disperse, heat to 110° C., reflux for 60 h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain sodium disulfonate-containing carbon nanotubes.
[0036] (5) Disperse 0.5 g of carbon nanotubes containing sodium bissulfonate in N,N-dimethylformamide solvent, add 20 g of PVDF, stir and mix for 2 h, let stand to degas, cast on a horizontal glass plate, and dry in an oven at 70°C to obtain an antistatic modified PVDF composite film.
[0037] Example 3
[0038] (1) 2 g of diaminobenzonitrile was added to an acetonitrile solvent, stirred and dispersed, and then 4.5 g of 1,3-propane sultone was added, and the temperature was raised to 85° C. and reacted for 20 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with acetone, and dried. The mixture was then added to deionized water, stirred and dispersed, and 4 g of sodium carbonate was added thereto. The mixture was reacted at 30° C. for 10 h. After the reaction was completed, the mixture was dried to obtain an intermediate 1.
[0039] (2) Under nitrogen conditions, intermediate 1 was added to methanol solvent, stirred and dispersed, and then 5% palladium carbon and 36% hydrochloric acid were added thereto. The reaction was stirred at 35°C for 48 hours. After the reaction was completed, the reaction was filtered, and the filtrate was distilled under reduced pressure and dried to obtain intermediate 2.
[0040] (3) Add 1 g of acidified carbon nanotubes and 120 mL of dichlorothionyl to N,N-dimethylformamide solvent, stir and disperse, heat to 105° C., reflux for 15 h, and after the reaction is completed, cool to room temperature, and filter under reduced pressure to obtain chlorinated carbon nanotubes.
[0041] (4) Disperse 1 g of acyl chloride carbon nanotubes in N,N-dimethylformamide solvent, add 10 g of intermediate 2 thereto, stir and disperse, heat to 100° C., reflux for 80 h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain sodium disulfonate-containing carbon nanotubes.
[0042] (5) Disperse 1 g of carbon nanotubes containing sodium bissulfonate in N,N-dimethylformamide solvent, add 20 g of PVDF, stir and mix for 4 h, let stand to degas, cast on a horizontal glass plate, and dry in an oven at 85°C to obtain an antistatic modified PVDF composite film.
[0043] Example 4
[0044] (1) Add 2 g of diaminobenzonitrile to acetonitrile solvent, stir and disperse, then add 4.2 g of 1,3-propane sultone, heat to 100° C., react for 24 h, and after the reaction is completed, cool to room temperature, filter, wash with acetone, and dry. Then add it to deionized water, stir and disperse, add 3.8 g of sodium carbonate, react at 35° C. for 15 h, and after the reaction is completed, dry to obtain intermediate 1.
[0045] (2) Under nitrogen conditions, intermediate 1 was added to methanol solvent, stirred and dispersed, and then 10% palladium carbon and 40% hydrochloric acid were added thereto. The reaction was stirred at 20°C for 50 hours. After the reaction was completed, the reaction was filtered, and the filtrate was distilled under reduced pressure and dried to obtain intermediate 2.
[0046] (3) Add 1 g of acidified carbon nanotubes and 80 mL of dichlorothionyl into N,N-dimethylformamide solvent, stir and disperse, heat to 100° C., reflux for 15 h, and after the reaction is completed, cool to room temperature, and filter under reduced pressure to obtain chlorinated carbon nanotubes.
[0047] (4) Disperse 1 g of acyl chloride carbon nanotubes in N,N-dimethylformamide solvent, add 8 g of intermediate 2 thereto, stir and disperse, heat to 105° C., reflux for 80 h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain sodium disulfonate-containing carbon nanotubes.
[0048] (5) Disperse 1.5 g of carbon nanotubes containing sodium bissulfonate in N,N-dimethylformamide solvent, add 20 g of PVDF, stir and mix for 3 h, let stand to degas, cast on a horizontal glass plate, and dry in an oven at 85°C to obtain an antistatic modified PVDF composite film.
[0049] Example 5
[0050] (1) 2 g of diaminobenzonitrile was added to an acetonitrile solvent, stirred and dispersed, and then 4.8 g of 1,3-propane sultone was added, and the temperature was raised to 90° C. and reacted for 24 h. After the reaction was completed, the mixture was cooled to room temperature, filtered, washed with acetone, and dried. The mixture was then added to deionized water, stirred and dispersed, and 4 g of sodium carbonate was added thereto. The mixture was reacted at 20° C. for 10 h. After the reaction was completed, the mixture was dried to obtain an intermediate 1.
[0051] (2) Under nitrogen conditions, intermediate 1 was added to methanol solvent, stirred and dispersed, and then 10% palladium carbon and 30% hydrochloric acid were added thereto. The reaction was stirred at 25°C for 35 hours. After the reaction was completed, the reaction was filtered, and the filtrate was distilled under reduced pressure and dried to obtain intermediate 2.
[0052] (3) Add 1 g of acidified carbon nanotubes and 100 mL of dichlorothionyl to N,N-dimethylformamide solvent, stir and disperse, heat to 110° C., reflux for 30 h, and after the reaction is completed, cool to room temperature, and filter under reduced pressure to obtain chlorinated carbon nanotubes.
[0053] (4) Disperse 1 g of acyl chloride carbon nanotubes in N,N-dimethylformamide solvent, add 10 g of intermediate 2 thereto, stir and disperse, heat to 105° C., reflux for 72 h, and after the reaction is completed, filter, wash with deionized water, and dry to obtain sodium disulfonate-containing carbon nanotubes.
[0054] (5) Disperse 2 g of carbon nanotubes containing sodium bissulfonate in N,N-dimethylformamide solvent, add 20 g of PVDF, stir and mix for 4 h, let stand to degas, cast on a horizontal glass plate, and dry in an oven at 75°C to obtain an antistatic modified PVDF composite film.
[0055] Comparative Example 1
[0056] The difference between this comparative example and Example 1 is that in step (5), multi-walled carbon nanotubes are used instead of carbon nanotubes containing sodium disulfonate.
[0057] Comparative Example 2
[0058] The difference between this comparative example and Example 1 is that in step (5), no carbon nanotubes containing sodium disulfonate are contained.
[0059] The tensile properties of PVDF composite films were tested using an electronic single yarn strength tester.
[0060] Use an electrostatic potentiometer to test the electrostatic potential.
[0061] Tensile strength / MPa Potential / kV Example 1 42.3 3.5 Example 2 45.6 2.8 Example 3 48.7 1.6 Example 4 47.5 1.4 Example 5 46.9 0.8 Comparative Example 1 40.8 4.9 Comparative Example 2 38.5 6.4
[0062] As can be seen from the table, the modified PVDF composite film prepared by the present invention has good mechanical properties, because Examples 1-5 contain carbon nanotubes containing sodium bissulfonate, which have a branched structure and a graphene structure, which can increase the mechanical properties of the PVDF film, while Comparative Example 1 does not contain a branched structure, so its mechanical properties are poor, and Comparative Example 2 does not contain carbon nanotubes containing sodium bissulfonate, so its mechanical properties are the worst. In addition, as can be seen from the above table, the PVDF composite film prepared by the present invention has good antistatic properties.
[0063] It should be understood that the above are only preferred embodiments of the present invention, and the patent scope of the present invention cannot be limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification, or directly or indirectly applied in other related fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing an antistatic modified PVDF composite film, characterized in that: The preparation method is as follows: (1) adding diaminobenzonitrile to an acetonitrile solvent, stirring and dispersing, then adding 1,3-propane sultone, heating to react, cooling to room temperature after the reaction is completed, filtering, washing with acetone, drying, then adding it to deionized water, stirring and dispersing, adding sodium carbonate thereto, reacting at 20-35° C. for 10-18 hours, and drying after the reaction is completed to obtain an intermediate 1; (2) Under nitrogen conditions, the intermediate 1 is added to a methanol solvent, stirred and dispersed, and then 5-10% palladium carbon and 30-40% hydrochloric acid are added thereto, and stirred for reaction. After the reaction is completed, the reaction is filtered, and the filtrate is distilled under reduced pressure and dried to obtain the intermediate 2; (3) adding the acidified carbon nanotubes and thionyl chloride to N,N-dimethylformamide solvent, stirring and dispersing, heating to 100-110° C., reflux reaction for 15-30 hours, cooling to room temperature after the reaction, and filtering under reduced pressure to obtain acyl chloride carbon nanotubes; (4) dispersing the acyl chloride carbon nanotubes in N,N-dimethylformamide solvent, adding intermediate 2 thereto, stirring and dispersing, heating to 100-110° C., reflux reaction for 60-80 hours, filtering after the reaction, washing with deionized water, and drying to obtain carbon nanotubes containing sodium disulfonate; (5) Dispersing the carbon nanotubes containing sodium bissulfonate in N,N-dimethylformamide solvent, adding PVDF thereto, stirring and mixing for 2-5 hours, standing to degas, casting on a horizontal glass plate to form a film, and drying in an oven to obtain an antistatic modified PVDF composite film.
2. The method for preparing the antistatic modified PVDF composite film according to claim 1, characterized in that: In the step (1), the usage ratio of diaminobenzonitrile, 1,3-propane sultone and sodium carbonate is 1 g:(2-2.4) g:(1.5-2) g.
3. The method for preparing the antistatic modified PVDF composite film according to claim 1, characterized in that: In the step (1), the temperature of the temperature-raising reaction is 80-100° C., and the reaction time is 12-24 hours.
4. The method for preparing the antistatic modified PVDF composite film according to claim 1, characterized in that: In the step (2), the stirring reaction time is 35-50 hours and the temperature is 20-35°C.
5. The method for preparing the antistatic modified PVDF composite film according to claim 1, characterized in that: In the step (3), the usage ratio of the acidified carbon nanotubes and the dichlorothionyl is 1 g: (80-120) mL.
6. The method for preparing the antistatic modified PVDF composite film according to claim 1, characterized in that: In the step (4), the usage ratio of the chlorinated carbon nanotubes and the intermediate 2 is 1 g:(5-12) g.
7. The method for preparing the antistatic modified PVDF composite film according to claim 1, characterized in that: In the step (5), the usage ratio of the sodium disulfonate carbon nanotubes and PVDF is (0.5-10) g:100 g.
8. The method for preparing the antistatic modified PVDF composite film according to claim 1, characterized in that: In the step (5), the temperature of the oven is 70-85°C.