A method for preparing a rare earth-based halide perovskite flexible film for X-ray detection

By adopting specific chemical weighing and heat treatment methods in the synthesis of rare earth-based halide Cs3EuCl6, the problems of low yield and unstable performance in the prior art were solved, and efficient and stable Cs3EuCl6/PDMS flexible films were successfully prepared, which is suitable for use in the process of In X-ray detection and lighting applications.

CN118562173BActive Publication Date: 2024-11-29HUBEI UNIV +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410985405.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-29
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

In the prior art, the synthesis method of the rare earth-based halide Cs3EuCl6 has problems such as low yield and easy reduction of Eu3+ to Eu2+ in raw materials, resulting in a decrease in energy conversion efficiency and performance matching.

Method used

The raw materials CsCl and EuCl3·6H2O were weighed by the molar mass percentage of the chemical formula Cs3EuCl6. After grinding, calcining and annealing, Cs3EuCl6 phosphor was obtained, and mixed with polydimethylsiloxane and curing agent and ultrasonic treatment was performed. The raw materials Cs3EuCl6 were spin-coated to form Cs3EuCl6. /PDMS flexible film.

Benefits of technology

It has achieved efficient preparation of rare earth-based halide Cs3EuCl6, improved yield, good crystal phase and stability of phosphors, and is suitable for X-ray irradiation measurement and solid-state lighting and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118562173B_ABST
    Figure CN118562173B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a rare earth halide perovskite flexible film for X-ray detection, which belongs to the field of X-ray radiation measurement and imaging technology. The present invention first adopts a low-temperature solid phase method to prepare a rare earth halide perovskite Cs3EuCl6 phosphor, then mixes the phosphor with polydimethylsiloxane and a curing agent, and spin-coats to prepare a Cs3EuCl6 / PDMS film. Compared with the synthesis method of rare earth halides reported in the literature, the preparation method described in the present invention has the advantages of simple preparation process, simple and easy to obtain raw materials, no need for inert gas protection under low-temperature synthesis, and high yield, which is suitable for large-scale production, thereby reducing equipment requirements and product production costs, and the obtained phosphor has good crystal phase and good stability. The Cs3EuCl6 phosphor and Cs3EuCl6 / PDMS film prepared by the present invention can be excited by ultraviolet-visible light and high-energy X-rays in the 250~466 nm band, and efficiently emit bright orange-red light, which is suitable for X-ray irradiation measurement, solid-state lighting and display and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of X-ray radiation measurement and imaging, and in particular to a method for preparing a rare earth-based halide perovskite flexible film for X-ray detection. Background Art

[0002] X-ray detection technology has a wide range of applications in medical diagnosis, industrial nondestructive testing, safety inspection, environmental monitoring, nuclear science and technology, space radiation detection and other fields. Compared with direct X-ray detectors, indirect detectors based on scintillators have the advantages of stability and economy. Scintillators can convert high-energy X-rays into low-energy visible light, and their physical properties directly affect X-ray detection and imaging effects. Due to the advantages of high light yield, high conversion efficiency, and low optical crosstalk, NaI:Tl, CsI:Tl and Bi4Ge3O 12 The commercial application of inorganic scintillators such as quartz crystals is relatively successful. However, these crystal materials usually face challenges such as high growth energy consumption, high growth process difficulty, heavy metal ion toxicity, and hygroscopic deliquescent properties. In addition, flexible scintillator screens can effectively distinguish spatially non-uniform X-rays, overcome imaging dead zones and spatial distortion caused by vignetting, and ensure efficient and accurate detection and imaging analysis of complex structures.

[0003] In recent years, halide perovskites can not only be prepared in large quantities at low temperature solutions and composited with flexible polymers, but also have outstanding advantages such as high X-ray absorption coefficient, high defect tolerance and high carrier mobility, and have attracted much attention in the field of flexible X-ray detectors. In particular, halide perovskites that replace Pb ions with rare earth ions have important application prospects in fields such as X-ray detection due to the large atomic number, absorption cross section, Stokes shift, high cutoff energy and excellent narrow-band emission of rare earth ions. Among them, the europium-based halide Cs3EuCl6, whose emission spectrum peak (616 nm) is highly matched with the optimal spectral response range (540~620 nm) of commercial silicon-based photoelectric sensors, is an ideal scintillator material. At present, the yield of Cs3EuCl6 nanocrystals prepared by hot injection is not high, and the oleylamine used in the synthesis easily makes part of Eu 3+ Reduction to Eu 2+ , which is prone to produce multi-band emission, resulting in a decrease in energy conversion efficiency and performance matching of silicon-based photoelectric sensors. Summary of the invention

[0004] The present invention aims to provide a method for preparing a rare earth-based halide perovskite flexible film for X-ray detection, so as to solve the problems existing in the above-mentioned prior art.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a rare earth-based halide perovskite flexible film for X-ray detection, comprising the following steps:

[0007] (1) weighing raw materials CsCl and EuCl3·6H2O according to the molar mass percentage in the chemical formula Cs3EuCl6, mixing the weighed CsCl and EuCl3·6H2O, adding anhydrous ethanol and grinding, and after the anhydrous ethanol evaporates, obtaining a mixed powder;

[0008] (2) calcining and annealing the mixed powder in sequence to obtain Cs3EuCl6 phosphor;

[0009] (3) Cs3EuCl6 phosphor, polydimethylsiloxane and a curing agent are mixed and then ultrasonically treated to obtain a colloidal precursor;

[0010] (4) Spin coating the colloidal precursor on a substrate and drying it to obtain a rare earth-based halide perovskite film Cs3EuCl6 / PDMS;

[0011] The calcination temperature is 450-550°C.

[0012] Furthermore, the calcination treatment time is 22-26 h, and the heating rate is 3-8°C / min.

[0013] Furthermore, the annealing temperature is 100-110° C., and the annealing time is 1-2 h.

[0014] Furthermore, the mass ratio of the Cs3EuCl6 phosphor, polydimethylsiloxane and curing agent is 1:1~1.2:0.1~0.2.

[0015] Furthermore, in the step (3), the mixing is carried out under vacuum conditions, the vacuum degree is 133 Pa, the mixing speed is 2500-3000 rpm, and the mixing time is 1-2 h.

[0016] Furthermore, the frequency of the ultrasonic treatment is 35-45 KHz, and the time of the ultrasonic treatment is 10-15 min.

[0017] Furthermore, the spin coating speed is 1800-2200 rpm, and the spin coating time is 20-40 s.

[0018] Furthermore, the drying temperature is 70-90° C., and the drying time is 4-6 h.

[0019] Beneficial effects of the present invention:

[0020] The Cs3EuCl6 phosphor and Cs3EuCl6 / PDMS film prepared by the present invention can be excited by X-rays and ultraviolet-visible light of 250-400 nm and 466 nm, emitting bright orange-red light, and are suitable for fields such as X-ray irradiation measurement, solid-state lighting and display. Compared with the method for synthesizing rare earth-based halides reported in the literature, the preparation method of the present invention has the advantages of simpler preparation process, simple and easy to obtain raw materials, no need for inert gas protection under low-temperature synthesis, high yield, etc., suitable for large-scale production, thereby reducing equipment requirements and product production costs, and the obtained phosphor has good crystal phase and good stability.

[0021] The Cs3EuCl6 / PDMS phosphor film of the present invention has the characteristics of low cost, safe operation and simple steps. The prepared phosphor film generates good orange-red light under near-ultraviolet excitation and has stable structure and stable luminescence. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 X-ray diffraction (XRD) spectra of Cs3EuCl6 phosphors synthesized at different temperatures.

[0023] Figure 2 This is the X-ray diffraction (XRD) spectrum of the Cs3EuCl6 phosphor prepared in Example 1.

[0024] Figure 3 This is the X-ray photoelectron spectroscopy (XPS) spectrum of the Eu 3d orbital in the Cs3EuCl6 phosphor prepared in Example 1.

[0025] Figure 4 This is the UV-Vis spectrum of the Cs3EuCl6 phosphor prepared in Example 1.

[0026] Figure 5 The fluorescence spectrum of the Cs3EuCl6 phosphor prepared in Example 1 ( =615nm, =324nm).

[0027] Figure 6 This is the CIE chromaticity coordinate diagram of the Cs3EuCl6 phosphor prepared in Example 1.

[0028] Figure 7 This is the X-ray absorption coefficient diagram of the Cs3EuCl6 phosphor prepared in Example 1.

[0029] Figure 8 X-ray spectra of the Cs3EuCl6 phosphor and Cs3EuCl6 / PDMS film prepared in Example 1.

[0030] Fig. 9This is the detection limit fitting diagram of the Cs3EuCl6 / PDMS film prepared in Example 1.

[0031] Fig.10 The actual picture and X-ray imaging picture of the Cs3EuCl6 / PDMS film prepared in Example 1.

[0032] Fig.11 This is a demonstration diagram of the flexibility of the Cs3EuCl6 / PDMS film prepared in Example 1. DETAILED DESCRIPTION

[0033] The present invention provides a method for preparing a rare earth-based halide perovskite flexible film for X-ray detection, comprising the following steps:

[0034] (1) weighing raw materials CsCl and EuCl3·6H2O according to the molar mass percentage in the chemical formula Cs3EuCl6, mixing the weighed CsCl and EuCl3·6H2O, adding anhydrous ethanol and grinding, and after the anhydrous ethanol evaporates, obtaining a mixed powder;

[0035] (2) calcining and annealing the mixed powder in sequence to obtain Cs3EuCl6 phosphor;

[0036] (3) Cs3EuCl6 phosphor, polydimethylsiloxane and a curing agent are mixed and then ultrasonically treated to obtain a colloidal precursor;

[0037] (4) Spin coating the colloidal precursor on a substrate and drying it to obtain a rare earth-based halide perovskite film Cs3EuCl6 / PDMS;

[0038] The calcination temperature is 450-550°C.

[0039] In the present invention, the calcination temperature is preferably 480-520°C, more preferably 500°C.

[0040] In the present invention, the calcination treatment time is 22-26 h, preferably 24 h; the heating rate is 3-8°C / min, preferably 5°C / min.

[0041] In the present invention, the annealing temperature is 100-110° C., preferably 110° C.; the annealing time is 1-2 h, preferably 1 h.

[0042] In the present invention, the mass ratio of the Cs3EuCl6 phosphor, polydimethylsiloxane and curing agent is 1:1~1.2:0.1~0.2, preferably 1:1:0.1.

[0043] In the present invention, the amount of anhydrous ethanol used is such that the raw materials CsCl and EuCl3·6H2O are mixed evenly.

[0044] In the present invention, the polydimethylsiloxane used is Sylgard 184 PDMS, and the curing agent used is a curing agent used in conjunction with Sylgard 184 PDMS.

[0045] In the present invention, in the step (3), the mixing is carried out under vacuum conditions, the vacuum degree is 133 Pa, the mixing speed is 2500-3000 rpm, preferably 2500 rpm, and the mixing time is 1-2 h, preferably 1 h.

[0046] In the present invention, the frequency of the ultrasonic treatment is 35-45 KHz, preferably 40 KHz, and the time of the ultrasonic treatment is 10-15 min, preferably 10 min.

[0047] In the present invention, the spin coating speed is 1800-2200 rpm, preferably 2000 rpm; the spin coating time is 20-40 s, preferably 30 s.

[0048] In the present invention, the drying temperature is 70-90° C., preferably 80° C.; the drying time is 4-6 h, preferably 5 h.

[0049] In the present invention, the analytical purity of the raw materials CsCl and EuCl3·6H2O is 99.99%.

[0050] The room temperature in the preparation method of the present invention is 20±5°C, preferably 20°C.

[0051] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0052] Example 1

[0053] According to the molar mass percentage in the chemical formula Cs3EuCl6, the raw materials CsCl (0.505 g) and EuCl3·6H2O (0.366 g) were weighed, and an appropriate amount of anhydrous ethanol was added to the raw materials and ground to make them uniformly mixed. After the anhydrous ethanol was completely volatilized, the sample was placed in an alumina crucible, and then placed in a muffle furnace and heated at a rate of 5°C / min. After the temperature was raised to 450°C, it was kept warm for 24 h. After naturally cooling to room temperature, the powder sample was ground to obtain a metastable Cs3EuCl6 phosphor. The metastable Cs3EuCl6 phosphor was then placed in a drying oven and annealed at 110°C for 1 h to obtain a Cs3EuCl6 phosphor sample. The obtained Cs3EuCl6 phosphor sample was ground with an agate grinding mortar for 10 min to obtain a preliminarily dispersed powder, and then further sieved with a 200-mesh fine sieve to obtain a particle-dispersed Cs3EuCl6 phosphor sample. Then, according to the mass ratio of 1:1:0.1, Cs3EuCl6 (0.5 g), PDMS (0.5 g) and curing agent (0.05 g) were weighed respectively, added with a magnetic rotor, stirred at 2500 rpm for 1 h in a vacuum atmosphere, and then placed in an ultrasonic machine for ultrasonic mixing at 40 kHz for 10 min. After Cs3EuCl6 and PDMS were evenly mixed, the obtained colloidal precursor was drop-coated on a glass slide with a rubber-tipped dropper, and spin-coated at 2000 rpm for 30 s in a vacuum atmosphere. Then, the spin-coated sample was placed in a drying oven and dried at 80°C for 5 h to obtain the above-mentioned Cs3EuCl6 / PDMS flexible film sample.

[0054] Example 2

[0055] Same as Example 1, except that the calcination temperature is 500°C.

[0056] Example 3

[0057] Same as Example 1, except that the calcination temperature is 550°C.

[0058] Comparative Example 1

[0059] Same as Example 1, except that the calcination temperature is 400°C.

[0060] Comparative Example 2

[0061] Same as Example 1, except that the calcination temperature is 600°C.

[0062] From the above examples, it can be seen that the present invention provides a method for preparing a rare earth-based halide perovskite flexible film for X-ray detection. The Cs3EuCl6 phosphors obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were tested. The XRD spectra of the Cs3EuCl6 phosphors at different reaction temperatures are shown in FIG. Figure 1As shown. It is observed that when the reaction temperature is 400℃, there are more impurity diffraction peaks in the spectrum, and pure Cs3EuCl6 phosphor cannot be obtained. Pure Cs3EuCl6 can be synthesized when the reaction temperature is increased to 450, 500 and 550℃. As the temperature is further increased to 600℃, the XRD spectrum shows that the high calcination temperature causes the crystal structure of Cs3EuCl6 phosphor to be destroyed, so the synthesis temperature range of the phosphor is 450~550℃.

[0063] The XRD spectrum of the Cs3EuCl6 phosphor obtained in Example 1 is as follows: Figure 2 It was observed that the peaks in the spectrum were sharp and free of impurity peaks, and could correspond one-to-one with the standard card, indicating that the Cs3EuCl6 phosphor sample of Example 1 was successfully obtained.

[0064] The Cs3EuCl6 phosphor obtained in Example 1 was subjected to XPS testing. The high-resolution XPS spectrum of Eu ions is shown in FIG. Figure 3 As shown. The binding energies of 1135 eV and 1165 eV are Eu 3+ 3D 5 / 2 Tracks and 3D 3 / 2 orbit, and no Eu 2+ The appearance of the orbitals proves that the purity of the phosphor is very high.

[0065] The absorption spectrum of the Cs3EuCl6 phosphor obtained in Example 1 was tested, and its UV-Vis absorption spectrum was as follows: Figure 4 As shown. Eu is shown at 380, 396, 415, 463 and 533 nm wavelengths. 3+ Characteristic absorption peaks of ions.

[0066] The fluorescence spectrum of the Cs3EuCl6 phosphor obtained in Example 1 was tested, and its excitation and emission spectra were as follows: Figure 5 As shown. Under the excitation of light with a wavelength of 324 nm, the phosphor emits bright orange-red light at 591 and 615 nm. There is no Eu between 400 and 700 nm. 2+ The characteristic emission peak appears.

[0067] The chromaticity spectrum of the Cs3EuCl6 phosphor obtained in Example 1 is calculated. Figure 6 As shown. By importing the emission spectrum data, the calculated chromaticity coordinates are (0.6289, 0.359), the dominant wavelength chromaticity coordinates are (0.643, 0.3579), the white light chromaticity coordinates are determined to be (0.33, 0.33), and the color purity is calculated to be 95.54% through the color purity formula. The color display is consistent with the actual luminescence.

[0068] The X-ray absorption coefficient of the Cs3EuCl6 phosphor obtained in Example 1 is compared. Figure 7 As shown, the absorption coefficient of Cs3EuCl6 is slightly higher than that of the commercial scintillator LYSO.

[0069] The Cs3EuCl6 phosphor and Cs3EuCl6 / PDMS film obtained in Example 1 were subjected to X-ray fluorescence testing, and the emission spectra thereof were as follows: Figure 8 As shown. Under the excitation of X-rays, the emission spectra of the phosphor Cs3EuCl6 and Cs3EuCl6 / PDMS film are Figure 5 The emission spectrum of the phosphor and the film is consistent, indicating that the luminescence mechanism of the phosphor and the film in Example 1 is the same as photoluminescence. After the phosphor is prepared into a film, its luminescence intensity is still high, which is 82.2% of the phosphor.

[0070] The X-ray detection limit test was performed on the Cs3EuCl6 / PDMS film obtained in Example 1. Fig. 9 As shown in the figure, the detection limit is about 4.84 uGy from the fitted curve. air / sec, lower than the medical detection limit of 5.5 uGy air / sec.

[0071] The Cs3EuCl6 / PDMS film obtained in Example 1 was subjected to an X-ray imaging test. Fig.10 As shown, Figure (a) is a physical picture of Cs3EuCl6 / PDMS film, and Figures (b) and (c) are physical pictures of X-ray imaging of Cs3EuCl6 / PDMS film.

[0072] The Cs3EuCl6 / PDMS film obtained in Example 1 was subjected to a Cs3EuCl6 / PDMS film flexibility test. Fig.11 As shown, Figure (a) and (b) show the film attached to the finger and the gel pen, and Figure (c) shows the film folded 360° and attached to the copper plate. The film shows good flexibility.

[0073] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a rare earth-based halide perovskite flexible film for X-ray detection, characterized in that: The following steps are involved: (1) weighing raw materials CsCl and EuCl3·6H2O according to the molar mass percentage in the chemical formula Cs3EuCl6, mixing the weighed CsCl and EuCl3·6H2O, adding anhydrous ethanol and grinding, and after the anhydrous ethanol evaporates, obtaining a mixed powder; (2) calcining and annealing the mixed powder in sequence to obtain Cs3EuCl6 phosphor; (3) Cs3EuCl6 phosphor, polydimethylsiloxane and a curing agent are mixed and then ultrasonically treated to obtain a colloidal precursor; (4) Spin coating the colloidal precursor on a substrate and drying it to obtain a rare earth-based halide perovskite film Cs3EuCl6 / PDMS; The calcination temperature is 450-550°C.

2. The method for preparing a rare earth-based halide perovskite flexible film for X-ray detection according to claim 1, characterized in that: The calcination treatment time is 22-26 h, and the heating rate is 3-8°C / min.

3. The method for preparing a rare earth-based halide perovskite flexible film for X-ray detection according to claim 1 or 2, characterized in that: The annealing temperature is 100-110° C., and the annealing time is 1-2 h.

4. The method for preparing a rare earth-based halide perovskite flexible film for X-ray detection according to claim 3, characterized in that: The mass ratio of the Cs3EuCl6 phosphor, polydimethylsiloxane and curing agent is 1:1~1.2:0.1~0.

2.

5. The method for preparing a rare earth-based halide perovskite flexible film for X-ray detection according to claim 1, characterized in that: In the step (3), the mixing is carried out under vacuum conditions, the vacuum degree is 133 Pa, the mixing speed is 2500-3000 rpm, and the mixing time is 1-2 h.

6. The method for preparing a rare earth-based halide perovskite flexible film for X-ray detection according to claim 1, 2 or 4, wherein the frequency of the ultrasonic treatment is 35-45 KHz, and the time of the ultrasonic treatment is 10-15 min.

7. The method for preparing a rare earth-based halide perovskite flexible film for X-ray detection according to claim 1, 2 or 4, characterized in that: The spin coating speed is 1800-2200 rpm, and the spin coating time is 20-40 s.

8. The method for preparing a rare earth-based halide perovskite flexible film for X-ray detection according to claim 1 or 2, characterized in that: The drying temperature is 70-90° C. and the drying time is 4-6 h.

Citation Information

Patent Citations

  • Novel lanthanide family lead-free perovskite nanocrystalline material and preparation method and application thereof

    CN114410303A

  • Preparation method of novel perovskite thin film as well as product and application of novel perovskite thin film

    CN114891254A

  • Low-dimensional perovskite-structured metal halide and preparation method and application thereof

    US20230235219A1