Bending-resistant sole material and preparation method thereof

By using polyurethane elastomer and nitrile rubber in sole materials, and by adding reinforced fillers and modified fibers, the shortcomings of existing sole materials in terms of wear resistance, mechanical properties and bending resistance are solved, achieving higher levels of strength wear resistance and mechanical properties.

CN118562282BActive Publication Date: 2024-11-22GUANGDONG YUESHENG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410801360.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-11-22
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

Existing sole materials have shortcomings in wear resistance, mechanical properties and bending resistance, especially in long-term use and multiple bending conditions.

Method used

Polyurethane elastomer and nitrile rubber are used as the main raw materials, and excellent mechanical properties are prepared by adding reinforced fillers such as CaCO3@MoS2 nanomaterials and modified fibers, combined with vulcanization agent and vulcanization accelerator, and hydrothermal reaction and surface modification technology are used to prepare sole material.

Benefits of technology

It significantly improves the wear resistance, mechanical properties and bending resistance of sole materials, enhances the low cost and environmentally friendly characteristics of fillers, and introduces modified fibers to improve the dispersion and cross-linking density of the materials, and improves the overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004903467870000101
    Figure BDA0004903467870000101
Patent Text Reader

Abstract

The present invention relates to the technical field of sole materials, and discloses a bending-resistant sole material and a preparation method thereof. The sole material prepared by the present invention comprises the following raw materials in parts by weight: 70-90 parts of polyurethane elastomer, 25-45 parts of nitrile rubber, 10-15 parts of polypropylene, 10-15 parts of reinforcing fillers, 2-4 parts of zinc oxide, 0.5-2 parts of antioxidant, 0.5-1 parts of ultraviolet absorber, 3-6 parts of silane coupling agent, 1-2 parts of vulcanizing agent, and 3-5 parts of vulcanization accelerator; it adopts polyurethane elastomer and nitrile rubber with excellent bending resistance as main raw materials, and then adds polypropylene and reinforcing fillers to further improve the bending resistance of substrate; wherein, reinforcing fillers can not only enhance the mechanical properties of substrate, but also improve the wear resistance of substrate; and the addition of polypropylene not only has good compatibility in substrate, but also can utilize its own excellent bending strength to further improve the bending resistance of substrate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sole materials, and in particular to a bending-resistant sole material and a preparation method thereof. Background Art

[0002] As people's living standards improve, the growth of the shoe material market has driven the demand for high-performance sole materials. Among them, the sole is the core part of the shoe, and its material and design directly affect the comfort, stability and overall performance of the shoe. The sole materials mainly include EVA, polyurethane elastomer, PVC and rubber soles. EVA soles are soft and highly elastic, but EVA soles are easy to absorb water, corrode and have poor durability; polyurethane elastomers are used as sole materials, with good toughness, hydrolysis resistance, chemical resistance and excellent elasticity, but according to different use environments, its anti-slip and wear resistance need to be improved; rubber soles have good wear resistance, anti-slip performance and folding resistance, but with the increase of actual demand, some properties of rubber soles, such as wear resistance, mechanical properties and elasticity, need to be modified to increase the wear resistance, mechanical properties and elasticity of the sole materials. In addition, since the soles of shoes will be bent many times during long-term use, the sole materials need to have excellent bending resistance.

[0003] In view of the advantages and disadvantages of polyurethane elastomer and rubber, a sole material with the common advantages of the two materials is designed, and additives are added to further improve the wear resistance, mechanical properties and bending resistance of the sole material. For example, the wear resistance, mechanical properties and bending resistance of the sole material can be improved by adding strong fillers (calcium carbonate, silica, etc.) or plant fibers with excellent mechanical properties. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a bending-resistant sole material and a preparation method thereof.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A bending-resistant sole material comprises the following raw materials in parts by weight: 70-90 parts of polyurethane elastomer, 25-45 parts of nitrile rubber, 10-15 parts of polypropylene, 10-15 parts of reinforcing filler, 2-4 parts of zinc oxide, 0.5-2 parts of antioxidant, 0.5-1 parts of ultraviolet absorber, 3-6 parts of silane coupling agent, 1-2 parts of vulcanizing agent, and 3-5 parts of vulcanization accelerator;

[0007] The reinforcing filler is prepared by the following steps:

[0008] Step A1, add thioacetamide and sodium molybdate into a beaker containing deionized water and stir evenly, add nano calcium carbonate and stir for 30 minutes, transfer the mixed solution into a reactor, and react at 180-220°C for 24 hours. After the reaction is completed, cool to room temperature, centrifuge, wash, and dry at 80°C for 12 hours to obtain CaCO3@MoS2 nanomaterials;

[0009] Further, the dosage ratio of thioacetamide, sodium molybdate, deionized water and nano-calcium carbonate is 0.3-0.9 g: 0.15-0.45 g: 60-90 mL: 0.1-0.3 g;

[0010] Step A2, add CaCO3@MoS2 nanomaterial, KH550, ethanol and deionized water into a flask and stir for 30 minutes, increase the system temperature to 55-75°C, continue stirring for 3-5 hours, after the reaction is completed, centrifuge, wash, collect the precipitate, redisperse in acetone and ultrasonicate for 1 hour, then control the system temperature at 0-5°C, add cyanuric chloride and triethylamine, stir and react for 3-5 hours, centrifuge, wash and dry to obtain the grafted modified CaCO3@MoS2 nanomaterial;

[0011] Further, the dosage ratio of CaCO3@MoS2 nanomaterial, KH550, ethanol, deionized water, acetone, cyanuric chloride and triethylamine is 2g: 0.01-0.02mol: 50mL: 10mL: 100mL: 0.01-0.02mol: 1.5-3.5g;

[0012] Step A3, 2-3g of modified fiber and 20mL of acetone are mixed evenly in a beaker, recorded as mixed solution A; 0.01-0.02mol of allylamine and 20mL of acetone are mixed evenly in a beaker, recorded as mixed solution B; the grafted modified CaCO3@MoS2 nanomaterial and acetone are added into the reactor and mixed evenly, then the mixed solution A is slowly added dropwise, and the system temperature is controlled to 40-50°C, and half of the 0.1mol / L sodium hydroxide solution is slowly added dropwise, and the reaction is carried out for 3-5h. After the reaction is completed, the temperature is continuously raised to 80-90°C, and the mixed solution B and the remaining sodium hydroxide solution are slowly added dropwise, and the reaction is continued for 4-7h. After the reaction is completed, centrifuge, wash, and dry to obtain a reinforced filler;

[0013] Furthermore, the usage ratio of the grafted modified CaCO3@MoS2 nanomaterial, acetone, mixed solution A, mixed solution B and sodium hydroxide solution is 2-3g:100mL:20mL:20mL:40-80mL.

[0014] The modified fiber is prepared by the following steps:

[0015] Step B1, soaking the plant fiber in a 15-30wt% sodium hydroxide solution, adjusting the system temperature to 30-40°C, and soaking for 1-2h to obtain pretreated plant fiber;

[0016] Further, the mass ratio of plant fiber to sodium hydroxide in the pretreated plant fiber is 1:30-80;

[0017] Step B2, dispersing the pretreated plant fiber in a flask containing deionized water, adjusting the pH to 7.5-8.5, adding dopamine hydrochloride, raising the system temperature to 30-40°C to react for 15-20h, and after the reaction is completed, filtering, washing, and drying to obtain modified fiber;

[0018] Furthermore, the dosage ratio of the pretreated plant fiber, deionized water and dopamine hydrochloride is 0.2-0.5 g:100 mL:0.06-0.15 g.

[0019] A method for preparing a bending-resistant sole material comprises the following steps:

[0020] Step S1, weighing raw materials by weight, kneading the nitrile rubber in an internal mixer for 3-5 minutes, then adding reinforcing filler, zinc oxide, antioxidant, ultraviolet absorber, silane coupling agent, vulcanizing agent and vulcanization accelerator, mixing evenly to obtain a premix, then extruding the premix through a rubber extruder at a temperature of 60-100° C., and then pelletizing to obtain rubber pellets;

[0021] Step S2, after the polyurethane elastomer, polypropylene and rubber particles are uniformly mixed, they are added into a twin-screw extruder, and dynamically vulcanized, extruded and granulated to obtain a bending-resistant sole material;

[0022] Furthermore, the twin-screw feeding zone is 175-185°C, the plasticizing zone is 180-190°C, the die head temperature is 195-205°C, and the screw speed is 120rpm.

[0023] Beneficial effects of the present invention:

[0024] The sole material prepared by the present invention adopts polyurethane elastomer and nitrile rubber with excellent bending resistance as main raw materials, and polypropylene and reinforcing filler are added to further improve the bending resistance of the matrix; wherein the reinforcing filler can not only enhance the mechanical properties of the matrix, but also improve the wear resistance of the matrix; and the addition of polypropylene not only has good compatibility in the matrix, but also can utilize its own excellent bending strength to further improve the bending resistance of the matrix.

[0025] The reinforcing filler is prepared by first selecting suitable sulfur source and molybdenum source as raw materials, and coating molybdenum disulfide on the surface of calcium carbonate by hydrothermal reaction to obtain CaCO3@MoS2 nanomaterial; then modifying the surface of the nanomaterial by a silane coupling agent to make it contain amino groups, and utilizing the amino groups on the surface to react with chlorine atoms in cyanuric chloride to obtain grafted modified CaCO3@MoS2 nanomaterial; finally, utilizing the remaining chlorine atoms in the grafted modified CaCO3@MoS2 nanomaterial to react with amino groups in modified fibers and allylamine to obtain a reinforcing filler. The reinforcing filler uses calcium carbonate as the base of the reinforcing filler, which has excellent mechanical properties and can effectively improve the strength and wear resistance of the matrix. At the same time, calcium carbonate also has the characteristics of low cost, non-toxicity, and environmental protection; the molybdenum disulfide coated on the surface of calcium carbonate has a lamellar structure similar to graphite, and the van der Waals force between the layers is weak and easy to slide, so it can provide self-lubrication with less friction in the matrix, thereby effectively improving the wear resistance of the matrix; the introduction of modified fibers improves the mechanical properties of the matrix, which is because the plant fibers have excellent flexibility, tensile strength and bending resistance. At the same time, the surface active groups of the plant fiber are exposed after being treated with alkali solution, which makes it have good modification properties. Therefore, dopamine hydrochloride is used as raw material and polydopamine is coated on its surface. The presence of polydopamine improves the dispersibility of the modified fiber, thereby enhancing the dispersibility of the reinforcing filler in the matrix, and further improving the mechanical properties, bending resistance, wear resistance and other comprehensive properties of the matrix; in addition, the allylamine introduced into the reinforcing filler makes it contain a double bond structure, which can participate in the subsequent vulcanization process, increase the crosslinking density of the matrix, and then improve the mechanical properties of the matrix. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] The modified fiber is prepared by the following steps:

[0029] Step B1, soaking 1g of bamboo fiber in 30g of 15wt% sodium hydroxide solution, adjusting the system temperature at 30°C, and soaking for 1h to obtain pretreated bamboo fiber;

[0030] Step B2, disperse 0.2g of pretreated bamboo fiber in a flask containing 100mL of deionized water, adjust the pH to 7.5, add 0.06g of dopamine hydrochloride, raise the system temperature to 30°C and react for 15h. After the reaction is completed, filter, wash and dry to obtain modified fiber.

[0031] The reinforcing filler is prepared by the following steps:

[0032] Step A1, add 0.3g thioacetamide and 0.15g sodium molybdate into a beaker containing 60mL deionized water and stir evenly, add 0.1g nano calcium carbonate and stir for 30min, transfer the mixed solution into a reactor, and react at 180°C for 24h. After the reaction is completed, cool to room temperature, centrifuge, wash, and dry at 80°C for 12h to obtain CaCO3@MoS2 nanomaterial;

[0033] Step A2, add 2g CaCO3@MoS2 nanomaterial, 0.01mol KH550, 50mL ethanol and 10mL deionized water into a flask and stir for 30min, raise the system temperature to 55°C, continue stirring for 3h, after the reaction is completed, centrifuge, wash, collect the precipitate, redisperse in 100mL acetone and ultrasonicate for 1h, then control the system temperature at 0°C, add 0.01mol cyanuric chloride and 1.5g triethylamine, stir and react for 3h, centrifuge, wash and dry to obtain the grafted modified CaCO3@MoS2 nanomaterial;

[0034] Step A3, mix 2g of modified fiber and 20mL of acetone in a beaker, record as mixed solution A; mix 0.01mol of allylamine and 20mL of acetone in a beaker, record as mixed solution B; add 2g of grafted modified CaCO3@MoS2 nanomaterial and 100mL of acetone into the reactor and mix evenly, then slowly add 20mL of mixed solution A, control the system temperature to 40℃, and slowly add 20mL of 0.1mol / L sodium hydroxide solution, react for 3h, after the reaction is completed, continue to increase the temperature to 80℃, slowly add 20mL of mixed solution B and 20mL of sodium hydroxide solution, continue to react for 4h, after the reaction is completed, centrifuge, wash, and dry to obtain reinforced filler.

[0035] Example 2

[0036] The modified fiber is prepared by the following steps:

[0037] Step B1, soaking 1g of bamboo fiber in 50g of 20wt% sodium hydroxide solution, adjusting the system temperature at 35°C, and soaking time for 1.5h to obtain pretreated bamboo fiber;

[0038] Step B2, disperse 0.35g of pretreated bamboo fiber in a flask containing 100mL of deionized water, adjust the pH to 8, add 0.1g of dopamine hydrochloride, raise the system temperature to 35°C and react for 17h. After the reaction is completed, filter, wash and dry to obtain modified fiber.

[0039] The reinforcing filler is prepared by the following steps:

[0040] Step A1, add 0.6g thioacetamide and 0.3g sodium molybdate into a beaker containing 75mL deionized water and stir evenly, add 0.2g nano calcium carbonate and stir for 30min, transfer the mixed solution into a reactor, and react at 200°C for 24h. After the reaction is completed, cool to room temperature, centrifuge, wash, and dry at 80°C for 12h to obtain CaCO3@MoS2 nanomaterial;

[0041] Step A2, add 2g CaCO3@MoS2 nanomaterial, 0.015mol KH550, 50mL ethanol and 10mL deionized water into a flask and stir for 30min, raise the system temperature to 65°C, continue stirring for 4h, after the reaction is completed, centrifuge, wash, collect the precipitate, redisperse in 100mL acetone and ultrasonicate for 1h, then control the system temperature at 0°C, add 0.015mol cyanuric chloride and 2.5g triethylamine, stir and react for 4h, centrifuge, wash and dry to obtain the grafted modified CaCO3@MoS2 nanomaterial;

[0042] Step A3, mix 2.5g of modified fiber and 20mL of acetone in a beaker, record as mixed solution A; mix 0.015mol of allylamine and 20mL of acetone in a beaker, record as mixed solution B; add 2.5g of grafted modified CaCO3@MoS2 nanomaterial and 100mL of acetone into the reactor and mix evenly, then slowly add 20mL of mixed solution A, control the system temperature to 45°C, and slowly add 30mL of 0.1mol / L sodium hydroxide solution, react for 4h, after the reaction is completed, continue to increase the temperature to 85°C, slowly add 20mL of mixed solution B and 30mL of sodium hydroxide solution, continue to react for 5h, after the reaction is completed, centrifuge, wash, and dry to obtain reinforced filler.

[0043] Example 3

[0044] The modified fiber is prepared by the following steps:

[0045] Step B1, soaking 1g of bamboo fiber in 80g of 30wt% sodium hydroxide solution, adjusting the system temperature at 40°C, and soaking for 2h to obtain pretreated bamboo fiber;

[0046] Step B2, disperse 0.5g of pretreated bamboo fiber in a flask containing 100mL of deionized water, adjust the pH to 8.5, add 0.15g of dopamine hydrochloride, raise the system temperature to 40°C and react for 20h. After the reaction is completed, filter, wash and dry to obtain modified fiber.

[0047] The reinforcing filler is prepared by the following steps:

[0048] Step A1, add 0.9g thioacetamide and 0.45g sodium molybdate into a beaker containing 90mL deionized water and stir evenly, add 0.3g nano calcium carbonate and stir for 30min, transfer the mixed solution into a reactor, and react at 220°C for 24h. After the reaction is completed, cool to room temperature, centrifuge, wash, and dry at 80°C for 12h to obtain CaCO3@MoS2 nanomaterial;

[0049] Step A2, add 2g CaCO3@MoS2 nanomaterial, 0.02mol KH550, 50mL ethanol and 10mL deionized water into a flask and stir for 30min, raise the system temperature to 75°C, continue stirring for 5h, after the reaction is completed, centrifuge, wash, collect the precipitate, redisperse in 100mL acetone and ultrasonicate for 1h, then control the system temperature at 0-5°C, add 0.02mol cyanuric chloride and 3.5g triethylamine, stir and react for 5h, centrifuge, wash and dry to obtain the grafted modified CaCO3@MoS2 nanomaterial;

[0050] Step A3, mix 3g of modified fiber and 20mL of acetone in a beaker, record as mixed solution A; mix 0.02mol of allylamine and 20mL of acetone in a beaker, record as mixed solution B; add 3g of grafted modified CaCO3@MoS2 nanomaterial and 100mL of acetone into the reactor and mix evenly, then slowly add 20mL of mixed solution A, control the system temperature to 50℃, and slowly add 40mL of 0.1mol / L sodium hydroxide solution, react for 5h, after the reaction is completed, continue to increase the temperature to 90℃, slowly add 20mL of mixed solution B and 40mL of sodium hydroxide solution, continue to react for 7h, after the reaction is completed, centrifuge, wash and dry to obtain reinforced filler.

[0051] Example 4

[0052] A method for preparing a bending-resistant sole material comprises the following steps:

[0053] 70 parts of polyurethane elastomer, 25 parts of nitrile rubber, 10 parts of polypropylene, 10 parts of reinforcing filler prepared in Example 1, 2 parts of zinc oxide, 0.5 parts of antioxidant 1010, 0.5 parts of ultraviolet absorber UV-1, 3 parts of KH560, 1 part of sulfur, and 3 parts of vulcanization accelerator TMTD;

[0054] Step S1, weighing raw materials by weight, kneading the nitrile rubber in an internal mixer for 3 minutes, then adding the reinforcing filler prepared in Example 1, zinc oxide, antioxidant 1010, ultraviolet absorber UV-1, KH560, sulfur and vulcanization accelerator TMTD, mixing evenly to obtain a premix, then extruding the premix through a rubber extruder at a temperature of 60° C., and then pelletizing to obtain rubber pellets;

[0055] Step S2, after the polyurethane elastomer, polypropylene and rubber particles are evenly mixed, they are added into a twin-screw extruder, dynamically vulcanized, extruded and granulated to obtain the bending-resistant sole material. The twin-screw feeding zone is 175°C, the plasticizing zone is 180°C, the head temperature is 195°C, and the screw speed is 120rpm.

[0056] Example 5

[0057] A method for preparing a bending-resistant sole material comprises the following steps:

[0058] 80 parts of polyurethane elastomer, 35 parts of nitrile rubber, 12 parts of polypropylene, 12 parts of reinforcing filler prepared in Example 2, 3 parts of zinc oxide, 10101 parts of antioxidant, 0.8 parts of ultraviolet absorber UV-1, 4 parts of KH560, 1.5 parts of sulfur, 4 parts of vulcanization accelerator TMTD;

[0059] Step S1, weighing raw materials by weight, kneading the nitrile rubber in an internal mixer for 4 minutes, adding the reinforcing filler prepared in Example 2, zinc oxide, antioxidant 1010, ultraviolet absorber UV-1, KH560, sulfur and vulcanization accelerator TMTD, mixing evenly to obtain a premix, and then extruding the premix through a rubber extruder at a temperature of 70° C., and then pelletizing to obtain rubber pellets;

[0060] Step S2: After the polyurethane elastomer, polypropylene and rubber particles are evenly mixed, they are added into a twin-screw extruder, dynamically vulcanized, extruded and granulated to obtain the bending-resistant sole material. The twin-screw feeding zone is 180° C., the plasticizing zone is 185° C., the head temperature is 200° C., and the screw speed is 120 rpm.

[0061] Example 6

[0062] A method for preparing a bending-resistant sole material comprises the following steps:

[0063] 90 parts of polyurethane elastomer, 45 parts of nitrile rubber, 15 parts of polypropylene, 15 parts of reinforcing filler prepared in Example 3, 4 parts of zinc oxide, 2 parts of antioxidant 1010, 1 parts of ultraviolet absorber UV-1, 6 parts of KH560, 2 parts of sulfur, and 5 parts of vulcanization accelerator TMTD;

[0064] Step S1, weighing raw materials by weight, kneading the nitrile rubber in an internal mixer for 5 minutes, then adding the reinforcing filler prepared in Example 3, zinc oxide, antioxidant 1010, ultraviolet absorber UV-1, KH560, sulfur and vulcanization accelerator TMTD, mixing evenly to obtain a premix, then extruding the premix through a rubber extruder at a temperature of 80° C., and then pelletizing to obtain rubber pellets;

[0065] Step S2: After the polyurethane elastomer, polypropylene and rubber particles are evenly mixed, they are added into a twin-screw extruder, dynamically vulcanized, extruded and granulated to obtain the bending-resistant sole material. The twin-screw feeding zone is 185°C, the plasticizing zone is 190°C, the head temperature is 205°C, and the screw speed is 120rpm.

[0066] Comparative Example 1

[0067] This comparative example is a sole material, which is different from Example 6 in that an equal amount of calcium carbonate is used to replace the reinforcing filler prepared in Example 3, and the rest are the same.

[0068] Comparative Example 2

[0069] This comparative example is a sole material, which is different from Example 6 in that an equal amount of bamboo fiber is used to replace the reinforcing filler prepared in Example 3, and the rest are the same.

[0070] Comparative Example 3

[0071] This comparative example is a sole material, which is different from Example 6 in that no polypropylene is added, and the rest are the same.

[0072] The performance tests of the sole materials prepared in Examples 4-6 and Comparative Examples 1-3 were performed:

[0073] Bending test: in accordance with GBT 3503.1-2015 "Footwear whole shoe test method folding performance";

[0074] Abrasion resistance test: in accordance with GB / T 5865-2008 "Determination of wear resistance of vulcanized rubber or thermoplastic rubber (rotating roller abrasion machine method)";

[0075] Mechanical properties test: tensile strength test was carried out in accordance with GB / T528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber"; the test results are shown in the following table:

[0076]

[0077] It can be seen from the above table that the sole material prepared by the present invention has excellent bending resistance, wear resistance and mechanical properties, and can be widely used in the production of soles.

[0078] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A bending-resistant sole material, characterized in that: The invention comprises the following raw materials in parts by weight: 70-90 parts of polyurethane elastomer, 25-45 parts of nitrile rubber, 10-15 parts of polypropylene, 10-15 parts of reinforcing filler, 2-4 parts of zinc oxide, 0.5-2 parts of antioxidant, 0.5-1 parts of ultraviolet absorber, 3-6 parts of silane coupling agent, 1-2 parts of vulcanizing agent and 3-5 parts of vulcanization accelerator; The reinforcing filler is prepared by the following steps: Step A1, add thioacetamide and sodium molybdate into a beaker containing deionized water and stir evenly, add nano calcium carbonate and stir for 30 minutes, transfer the mixed solution into a reactor, and react at 180-220°C for 24 hours. After the reaction is completed, cool to room temperature, centrifuge, wash, and dry at 80°C for 12 hours to obtain CaCO3@MoS2 nanomaterials; Step A2, add CaCO3@MoS2 nanomaterial, KH550, ethanol and deionized water into a flask and stir for 30 minutes, increase the system temperature to 55-75°C, continue stirring for 3-5 hours, after the reaction is completed, centrifuge, wash, collect the precipitate, redisperse in acetone and ultrasonicate for 1 hour, then control the system temperature at 0-5°C, add cyanuric chloride and triethylamine, stir and react for 3-5 hours, centrifuge, wash and dry to obtain the grafted modified CaCO3@MoS2 nanomaterial; Step A3, 2-3g of modified fiber and 20mL of acetone are mixed evenly in a beaker, recorded as mixed solution A; 0.01-0.02mol of allylamine and 20mL of acetone are mixed evenly in a beaker, recorded as mixed solution B; the grafted modified CaCO3@MoS2 nanomaterial and acetone are added into the reactor and mixed evenly, then the mixed solution A is slowly added dropwise, and the system temperature is controlled to 40-50°C, and half of the 0.1mol / L sodium hydroxide solution is slowly added dropwise, and the reaction is carried out for 3-5h. After the reaction is completed, the temperature is continuously raised to 80-90°C, and the mixed solution B and the remaining sodium hydroxide solution are slowly added dropwise, and the reaction is continued for 4-7h. After the reaction is completed, centrifuge, wash, and dry to obtain a reinforced filler; The modified fiber is prepared by the following steps: Step B1, soaking the plant fiber in a 15-30wt% sodium hydroxide solution, adjusting the system temperature to 30-40°C, and soaking for 1-2h to obtain pretreated plant fiber; Step B2, disperse the pretreated plant fiber in a flask containing deionized water, adjust the pH to 7.5-8.5, add dopamine hydrochloride, increase the system temperature to 30-40°C and react for 15-20 hours. After the reaction is completed, filter, wash and dry to obtain modified fiber.

2. The bending-resistant sole material according to claim 1, characterized in that: In step A1, the usage ratio of thioacetamide, sodium molybdate, deionized water and nano calcium carbonate is 0.3-0.9 g: 0.15-0.45 g: 60-90 mL: 0.1-0.3 g.

3. The bending-resistant sole material according to claim 1, characterized in that: In step A2, the dosage ratio of CaCO3@MoS2 nanomaterial, KH550, ethanol, deionized water, acetone, cyanuric chloride and triethylamine is 2g:0.01-0.02mol:50mL:10mL:100mL:0.01-0.02mol:1.5-3.5g.

4. The bending-resistant sole material according to claim 1, characterized in that: In step A3, the usage ratio of the grafted modified CaCO3@MoS2 nanomaterial, acetone, mixed solution A, mixed solution B and sodium hydroxide solution is 2-3g:100mL:20mL:20mL:40-80mL.

5. The bending-resistant sole material according to claim 1, characterized in that: Furthermore, in step B1, the mass ratio of plant fiber to sodium hydroxide in the pretreated plant fiber is 1:30-80.

6. The bending-resistant sole material according to claim 1, characterized in that: In step B2, the dosage ratio of the pretreated plant fiber, deionized water and dopamine hydrochloride is 0.2-0.5 g:100 mL:0.06-0.15 g.

7. The method for preparing a bending-resistant sole material according to claim 1, characterized in that: The following steps are involved: Step S1, weighing raw materials by weight, kneading the nitrile rubber in an internal mixer for 3-5 minutes, then adding reinforcing filler, zinc oxide, antioxidant, ultraviolet absorber, silane coupling agent, vulcanizing agent and vulcanization accelerator, mixing evenly to obtain a premix, then extruding the premix through a rubber extruder at a temperature of 60-100° C., and then pelletizing to obtain rubber pellets; Step S2, after the polyurethane elastomer, polypropylene and rubber particles are evenly mixed, they are added into a twin-screw extruder, dynamically vulcanized, extruded and granulated to obtain the bending-resistant sole material. The twin-screw feeding zone is 175-185°C, the plasticizing zone is 180-190°C, the head temperature is 195-205°C, and the screw speed is 120rpm.