A kind of outdoor polyurethane simulated wood grain material and preparation method thereof
Through the three-layer structure of polyurethane simulated wood grain material and self-made silicone mold technology, the problems of unrealistic appearance and poor weather resistance of traditional polyurethane materials are solved, achieving a realistic wood grain appearance and high weather resistance, and extending the outdoor service life.
Patent Information
- Application Number
- CN202411025259.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Traditional polyurethane materials do not have a realistic appearance when used outdoors, have poor weather resistance, and are prone to aging, making it difficult to meet the needs of high-quality outdoor materials.
It adopts a three-layer structure of polyurethane simulated wood grain material, which is composed of an outer layer, a modified layer and a main layer. The outer layer is composed of polyether polyol, isocyanate and modified HDI trimer, and the modified layer contains polyol, 1,4- Butylene glycol, antioxidants, light stabilizers and pigments, the main layer contains polyol, 1,4-butanediol, water, antioxidants, light stabilizers, surfactants and inorganic fillers, through homemade silicone with wood texture The mold is formed.
It achieves the realistic wood grain appearance of polyurethane materials, enhances weather resistance and anti-aging performance, extends outdoor service life, and avoids the problems of fading, yellowing and wood grain patches falling off.
Smart Images

Figure CN118562287B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite material preparation, and more specifically discloses an outdoor polyurethane simulated wood grain material and a preparation method thereof. Background Art
[0002] With the rapid development of the construction, furniture and decoration industries, higher and higher requirements are placed on the aesthetics, durability and environmental protection of materials. Polyurethane materials have been widely used in various fields due to their excellent physical properties and processability. When used outdoors, the appearance of the polyurethane material needs to be made into wood grain so that the polyurethane material can better blend with the natural environment. The traditional practice is to paste wood grain patches on the surface of the polyurethane material, resulting in an appearance that is not realistic enough, and long-term outdoor use can easily cause the appearance to fade and turn yellow, which further leads to distortion. In addition, when traditional polyurethane materials are used outdoors, they often face problems such as poor weather resistance and easy aging, which makes it difficult to meet the market demand for high-quality outdoor materials. Summary of the invention
[0003] The main technical problem solved by the present invention is to provide an outdoor polyurethane simulated wood grain material and a preparation method thereof, which can solve the problem that the traditional polyurethane material has an insufficiently realistic appearance and poor weather resistance and is easy to age.
[0004] To solve the above technical problems, according to one aspect of the present invention, more specifically, an outdoor polyurethane simulated wood grain material is provided, which is composed of an outer layer, a finishing layer and a main body layer, wherein:
[0005] The outer layer is composed of two components, wherein component A includes: polyether polyol, diisocyanate, hydrophilic chain extender, and component B includes: modified HDI trimer;
[0006] The modification layer is composed of two components, wherein component A includes: polyol and diisocyanate, and component B includes: polyol, 1,4-butanediol, antioxidant, light stabilizer, surfactant and pigment;
[0007] The main layer is composed of three components, among which component A includes: polyol, diisocyanate, component B includes: polyol, 1,4-butanediol, water, antioxidant, light stabilizer, surfactant and pigment, inorganic filler, and component C includes: reinforcing fiber, polyhydroxyacetate, nickel-1,2-dithiobenzothiadiazole coordination polymer.
[0008] Furthermore, the component B in the modification layer specifically includes the following components in parts by weight: 100 parts of polyol, 0.5-5 parts of 1,4-butanediol, 0.1-0.3 parts of antioxidant, 0.3-1.0 parts of light stabilizer, 0.3-3.0 parts of surfactant and pigment;
[0009] The B component in the main layer specifically includes the following components in parts by weight: 100 parts of polyol, 0.5-5 parts of 1,4-butanediol, 0.02-1 parts of water, 0.1-0.3 parts of antioxidant, 0.3-1.0 parts of light stabilizer, 0.3-3.0 parts of surfactant and pigment, 1-10 parts of inorganic filler, and the C component specifically includes the following components in parts by weight: 8-12 parts of reinforcing fiber, 1-3 parts of polyhydroxy acetate, and 0.5-2.5 parts of nickel-1,2-dithiobenzothiadiazole coordination polymer.
[0010] Furthermore, the A component of the outer layer is prepared by mixing and heating a polyether polyol, a diisocyanate and a hydrophilic chain extender, the A component of the modification layer is prepared by mixing and heating a polyol and a diisocyanate, and its NCO value is 3.0-9.0%, and the A component of the main layer is prepared by mixing and heating a polyol and a diisocyanate, and its NCO value is 3.0-11.0%.
[0011] Furthermore, the modified HDI trimer is composed of HDI trimer, polytetrafluoroethylene, graphene oxide and polyetheretherketone, and is specifically prepared as follows: HDI trimer, polytetrafluoroethylene and polyetheretherketone are mixed in a ratio of 5:3:1 to form a mixture, and then aged at 35-40°C for 10-15min, and then 1 / 3 of the mass of the mixture The graphene oxide is added to the mixture, and after fully stirring and mixing, the modified HDI trimer is obtained.
[0012] Furthermore, the preparation process of the reinforcing fiber is: firstly, the glass fiber and the modified aramid fiber are twisted in a ratio of 1:2 to form a fiber twisted wire, and then a cross-linking agent is sprayed on the surface of the fiber twisted wire, and the reinforcing fiber is obtained after drying.
[0013] Furthermore, the preparation process of the modified aramid fiber is as follows: the aramid fiber is hot-melted at 560-600°C to form an aramid fiber melt, and then nano-silicon oxide with a particle size of 10-20nm is added to the aramid fiber melt, and the ratio of the aramid fiber melt to the nano-silicon oxide is 3:1. After mixing evenly, the aramid fiber melt is placed in a spinner, and extruded through the spinneret to form a melt stream with a diameter of 70-100nm, and then the melt stream is cooled to form a modified aramid fiber.
[0014] According to another aspect of the present invention, there is provided a method for preparing an outdoor polyurethane simulated wood grain material, comprising the following steps:
[0015] S1. Making of silicone mold with wood grain: select wood with clear grain and suitable size, dry it, spray the release agent, and then pour room temperature vulcanized silicone rubber on the surface. After 24 hours of aging, demoulding can produce a silicone mold with wood grain on one side;
[0016] S2. Preparation of the outer layer of polyurethane simulated wood grain material: placing the silicone mold in a mold frame and heating it, with the wood grain side facing upward, spraying a release agent on the surface, and then evenly mixing the AB components of the outer layer according to a certain proportion, and applying them to the grain surface of the silicone mold by spraying or brushing to obtain the outer layer of polyurethane simulated wood grain material;
[0017] S3, preparation of polyurethane simulated wood grain material modification layer: after mixing the AB components of the modification layer evenly in proportion, apply them to the outer layer of the polyurethane simulated wood grain material by spraying or scraping to prepare the polyurethane simulated wood grain material modification layer;
[0018] S4, preparation of the main layer of polyurethane simulated wood grain material: after the ABC components of the main layer are mixed evenly in proportion, they are applied on the polyurethane simulated wood grain material modification layer by spraying or scraping to prepare the main layer of polyurethane simulated wood grain material;
[0019] S5. Demolding of finished product: After the maturation of each layer is completed, the product is removed from the silicone mold as a whole, so that the polyurethane simulated wood grain material can be obtained.
[0020] Furthermore, the wood in step S1 is made by weathered wood, carbonized wood or roughened wood.
[0021] Furthermore, in step S1, the thickness of the room temperature vulcanized silicone rubber poured on the wood surface is 3-10 mm.
[0022] The beneficial effects of the outdoor polyurethane simulated wood grain material and the preparation method thereof are as follows: by making a silicone mold with wood grains by yourself, and molding the homemade raw materials in the silicone mold with wood grains, the prepared polyurethane material can have a realistic wood grain appearance, and compared with the traditional method of directly pasting wood grain patches on polyurethane materials, the polyurethane material can be prevented from being used outdoors for a long time, resulting in the appearance fading and yellowing, and the wood grain patches falling off, thereby causing the appearance to be distorted. In addition, the three-layer structure of the material is obtained by using homemade raw materials, which can ensure that the material has stronger weather resistance and anti-aging performance during outdoor use, thereby giving it a longer outdoor service life and avoiding aging and brittleness during a shorter outdoor use period. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention is further described in detail below with reference to the accompanying drawings and specific implementation methods.
[0024] Figure 1 This is a silicone mold image with wood texture;
[0025] Figure 2 To prepare each layer of polyurethane simulated wood grain material diagram;
[0026] Figure 3 This is the finished product picture of polyurethane simulated wood grain material;
[0027] Figure 4 This is a partial picture of the polyurethane simulated wood grain material. DETAILED DESCRIPTION
[0028] The present invention will be described in detail below with reference to the accompanying drawings and in combination with embodiments. It should be noted that the embodiments and features in the embodiments of the present application can be combined with each other without conflict.
[0029] A polyurethane simulated wood grain material for outdoor use, comprising an outer layer, a finishing layer and a main body layer. The specific preparation process of the material is as follows:
[0030] (1) Select wood with clear texture and appropriate size (made by weathered wood, carbonized wood or roughened wood), dry it, spray the release agent on it, and then pour 3-10mm thick room temperature vulcanized silicone rubber on the surface. After 24 hours of aging, demolding can produce a silicone mold with wood texture on one side.
[0031] (2) Place the silicone mold in a mold frame and heat it, with the wood grain side facing upward, and spray a release agent on its surface. Then, mix the components of the outer layer evenly in proportion, and apply them to the texture surface of the silicone mold by spraying or brushing to obtain the outer layer of polyurethane simulated wood grain material.
[0032] (3) After the components of the modification layer are mixed evenly in proportion, they are applied to the outer layer of the polyurethane simulated wood grain material by spraying or scraping to obtain the polyurethane simulated wood grain material modification layer.
[0033] (4) After the components of the main layer are mixed evenly in proportion, they are coated on the polyurethane simulated wood grain material modification layer by spraying or scraping to obtain the polyurethane simulated wood grain material main layer.
[0034] (5) After all layers have been matured, the product is removed from the silicone mold as a whole, thereby obtaining a polyurethane simulated wood grain material.
[0035] Embodiment 1
[0036] The outer layer component A is prepared by mixing and heating polyether polyol, diisocyanate and hydrophilic chain extender. The outer layer component B is formed by mixing HDI trimer, polytetrafluoroethylene and polyetheretherketone in a ratio of 5:3:1, then aging at 35°C for 10 minutes, and then adding 1 / 3 of the mixture mass of graphene oxide into the mixture, and stirring and mixing thoroughly to obtain a modified HDI trimer.
[0037] The A component of the modification layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 3.0%. The B component of the modification layer is composed of 100 parts of polyol, 0.5 parts of 1,4-butanediol, 0.1 parts of antioxidant, 0.3 parts of light stabilizer, 0.3 parts of surfactant and pigment.
[0038] The A component of the main layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 3.0%. The B component of the main layer is composed of 100 parts of polyol, 0.5 parts of 1,4-butanediol, 0.02 parts of water, 0.1 parts of antioxidant, 0.3 parts of light stabilizer, 0.3 parts of surfactant and pigment, and 1 part of inorganic filler. The C component of the main layer is composed of 8 parts of reinforcing fiber, 1 part of polyhydroxyacetate, and 0.5 parts of nickel-1,2-dithiobenzothiadiazole coordination polymer. Among them:
[0039] The reinforcing fiber is obtained by twisting glass fiber and modified aramid fiber in a ratio of 1:2 to form fiber twisted wire, spraying a crosslinking agent on the surface of the fiber twisted wire, and drying it.
[0040] The modified aramid fiber is prepared by hot-melting the aramid fiber at 560°C to form an aramid fiber melt, and then adding nano-silicon oxide with a particle size of 10 nm to the aramid fiber melt. The ratio of the aramid fiber melt to the nano-silicon oxide is 3:1. After mixing evenly, the aramid fiber melt is put into a spinner, extruded through the spinneret to form a melt stream with a diameter of 70 nm, and then the melt stream is cooled to obtain the modified aramid fiber.
[0041] Embodiment 2
[0042] The outer layer component A is prepared by mixing and heating polyether polyol, diisocyanate and hydrophilic chain extender. The outer layer component B is formed by mixing HDI trimer, polytetrafluoroethylene and polyetheretherketone in a ratio of 5:3:1, then aging at 37°C for 13 minutes, and then adding 1 / 3 of the mixture by mass of graphene oxide into the mixture, and stirring and mixing thoroughly to obtain a modified HDI trimer.
[0043] The A component of the modification layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 5.6%. The B component of the modification layer is composed of 100 parts of polyol, 3.2 parts of 1,4-butanediol, 0.2 parts of antioxidant, 0.6 parts of light stabilizer, 2.1 parts of surfactant and pigment.
[0044] The A component of the main layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 7.0%. The B component of the main layer is composed of 100 parts of polyol, 3.4 parts of 1,4-butanediol, 0.36 parts of water, 0.2 parts of antioxidant, 0.5 parts of light stabilizer, 1.8 parts of surfactant and pigment, and 7 parts of inorganic filler. The C component of the main layer is composed of 10 parts of reinforcing fiber, 2 parts of polyhydroxyacetate, and 1.6 parts of nickel-1,2-dithiobenzothiadiazole coordination polymer. Among them:
[0045] The reinforcing fiber is obtained by twisting glass fiber and modified aramid fiber in a ratio of 1:2 to form fiber twisted wire, spraying a crosslinking agent on the surface of the fiber twisted wire, and drying it.
[0046] The modified aramid fiber is prepared by hot-melting the aramid fiber at 580°C to form an aramid fiber melt, and then adding nano-silicon oxide with a particle size of 15 nm to the aramid fiber melt. The ratio of the aramid fiber melt to the nano-silicon oxide is 3:1. After mixing evenly, the aramid fiber melt is put into a spinner, extruded through the spinneret to form a melt stream with a diameter of 90 nm, and then the melt stream is cooled to obtain the modified aramid fiber.
[0047] Embodiment 3
[0048] The outer layer component A is prepared by mixing and heating polyether polyol, diisocyanate and hydrophilic chain extender. The outer layer component B is formed by mixing HDI trimer, polytetrafluoroethylene and polyetheretherketone in a ratio of 5:3:1, then aging at 40°C for 15 minutes, and then adding 1 / 3 of the mixture mass of graphene oxide into the mixture, and stirring and mixing thoroughly to obtain a modified HDI trimer.
[0049] The A component of the modification layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 9.0%. The B component of the modification layer is composed of 100 parts of polyol, 5 parts of 1,4-butanediol, 0.3 parts of antioxidant, 1.0 parts of light stabilizer, 3.0 parts of surfactant and pigment.
[0050] The A component of the main layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 11.0%. The B component of the main layer is composed of 100 parts of polyol, 5 parts of 1,4-butanediol, 1 part of water, 0.3 parts of antioxidant, 1.0 parts of light stabilizer, 3.0 parts of surfactant and pigment, and 10 parts of inorganic filler. The C component of the main layer is composed of 12 parts of reinforcing fiber, 3 parts of polyhydroxyacetate, and 2.5 parts of nickel-1,2-dithiobenzothiadiazole coordination polymer. Among them:
[0051] The reinforcing fiber is obtained by twisting glass fiber and modified aramid fiber in a ratio of 1:2 to form fiber twisted wire, spraying a crosslinking agent on the surface of the fiber twisted wire, and drying it.
[0052] The modified aramid fiber is prepared by hot-melting the aramid fiber at 600°C to form an aramid fiber melt, and then adding nano-silicon oxide with a particle size of 20 nm to the aramid fiber melt. The ratio of the aramid fiber melt to the nano-silicon oxide is 3:1. After mixing evenly, the aramid fiber melt is put into a spinner, extruded through the spinneret to form a melt stream with a diameter of 100 nm, and then the melt stream is cooled to obtain the modified aramid fiber.
[0053] Comparative Example 1
[0054] The outer layer component A is prepared by mixing and heating polyether polyol, diisocyanate and hydrophilic chain extender. The outer layer component B is formed by mixing HDI trimer, polytetrafluoroethylene and polyetheretherketone in a ratio of 5:3:1, then aging at 40°C for 15 minutes, and then adding 1 / 3 of the mixture mass of graphene oxide into the mixture, and stirring and mixing thoroughly to obtain a modified HDI trimer.
[0055] The modifying layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 9.0%.
[0056] The A component of the main layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 11.0%. The B component of the main layer is composed of 100 parts of polyol, 5 parts of 1,4-butanediol, 1 part of water, 0.3 parts of antioxidant, 1.0 parts of light stabilizer, 3.0 parts of surfactant and pigment, and 10 parts of inorganic filler. The C component of the main layer is composed of 12 parts of reinforcing fiber, 3 parts of polyhydroxyacetate, and 2.5 parts of nickel-1,2-dithiobenzothiadiazole coordination polymer. Among them:
[0057] The reinforcing fiber is obtained by twisting glass fiber and modified aramid fiber in a ratio of 1:2 to form fiber twisted wire, spraying a crosslinking agent on the surface of the fiber twisted wire, and drying it.
[0058] The modified aramid fiber is prepared by hot-melting the aramid fiber at 600°C to form an aramid fiber melt, and then adding nano-silicon oxide with a particle size of 20 nm to the aramid fiber melt. The ratio of the aramid fiber melt to the nano-silicon oxide is 3:1. After mixing evenly, the aramid fiber melt is put into a spinner, extruded through the spinneret to form a melt stream with a diameter of 100 nm, and then the melt stream is cooled to obtain the modified aramid fiber.
[0059] Comparative Example 2
[0060] The outer layer component A is prepared by mixing and heating polyether polyol, diisocyanate and hydrophilic chain extender. The outer layer component B is formed by mixing HDI trimer, polytetrafluoroethylene and polyetheretherketone in a ratio of 5:3:1, then aging at 40°C for 15 minutes, and then adding 1 / 3 of the mixture mass of graphene oxide into the mixture, and stirring and mixing thoroughly to obtain a modified HDI trimer.
[0061] The A component of the modification layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 9.0%. The B component of the modification layer is composed of 100 parts of polyol, 5 parts of 1,4-butanediol, 0.3 parts of antioxidant, 1.0 parts of light stabilizer, 3.0 parts of surfactant and pigment.
[0062] The A component of the main layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 11.0%. The B component of the main layer is composed of 12 parts of reinforcing fiber, 3 parts of polyhydroxyacetic acid ester, and 2.5 parts of nickel-1,2-dithiobenzothiadiazole coordination polymer. Among them:
[0063] The reinforcing fiber is obtained by twisting glass fiber and modified aramid fiber in a ratio of 1:2 to form fiber twisted wire, spraying a crosslinking agent on the surface of the fiber twisted wire, and drying it.
[0064] The modified aramid fiber is prepared by hot-melting the aramid fiber at 600°C to form an aramid fiber melt, and then adding nano-silicon oxide with a particle size of 20 nm to the aramid fiber melt. The ratio of the aramid fiber melt to the nano-silicon oxide is 3:1. After mixing evenly, the aramid fiber melt is put into a spinner, extruded through the spinneret to form a melt stream with a diameter of 100 nm, and then the melt stream is cooled to obtain the modified aramid fiber.
[0065] Comparative Example 3
[0066] The outer layer component A is prepared by mixing and heating polyether polyol, diisocyanate and hydrophilic chain extender. The outer layer component B is formed by mixing HDI trimer, polytetrafluoroethylene and polyetheretherketone in a ratio of 5:3:1, then aging at 40°C for 15 minutes, and then adding 1 / 3 of the mixture mass of graphene oxide into the mixture, and stirring and mixing thoroughly to obtain a modified HDI trimer.
[0067] The A component of the modification layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 9.0%. The B component of the modification layer is composed of 100 parts of polyol, 5 parts of 1,4-butanediol, 0.3 parts of antioxidant, 1.0 parts of light stabilizer, 3.0 parts of surfactant and pigment.
[0068] The A component of the main layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 11.0%. The B component of the main layer is composed of 100 parts of polyol, 5 parts of 1,4-butanediol, 1 part of water, 0.3 parts of antioxidant, 1.0 parts of light stabilizer, 3.0 parts of surfactant and pigment, and 10 parts of inorganic filler.
[0069] Comparative Example 4
[0070] The outer layer is prepared by mixing polyether polyol, diisocyanate and hydrophilic chain extender and heating them for reaction.
[0071] The A component of the modification layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 9.0%. The B component of the modification layer is composed of 100 parts of polyol, 5 parts of 1,4-butanediol, 0.3 parts of antioxidant, 1.0 parts of light stabilizer, 3.0 parts of surfactant and pigment.
[0072] The A component of the main layer is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 11.0%. The B component of the main layer is composed of 100 parts of polyol, 5 parts of 1,4-butanediol, 1 part of water, 0.3 parts of antioxidant, 1.0 parts of light stabilizer, 3.0 parts of surfactant and pigment, and 10 parts of inorganic filler. The C component of the main layer is composed of 12 parts of reinforcing fiber, 3 parts of polyhydroxyacetate, and 2.5 parts of nickel-1,2-dithiobenzothiadiazole coordination polymer. Among them:
[0073] The reinforcing fiber is obtained by twisting glass fiber and modified aramid fiber in a ratio of 1:2 to form fiber twisted wire, spraying a crosslinking agent on the surface of the fiber twisted wire, and drying it.
[0074] The modified aramid fiber is prepared by hot-melting the aramid fiber at 600°C to form an aramid fiber melt, and then adding nano-silicon oxide with a particle size of 20 nm to the aramid fiber melt. The ratio of the aramid fiber melt to the nano-silicon oxide is 3:1. After mixing evenly, the aramid fiber melt is put into a spinner, extruded through the spinneret to form a melt stream with a diameter of 100 nm, and then the melt stream is cooled to obtain the modified aramid fiber.
[0075] Comparative Example 5
[0076] Wood grain patches are pasted on the surface of JYJB42-333-1000 polyurethane material by white latex to form outdoor polyurethane reverse wood grain material.
[0077] The outdoor polyurethane simulated wood grain materials prepared in Examples 1 to 3 and the outdoor polyurethane simulated wood grain materials prepared in Comparative Examples 1 to 5 were exposed to simulated outdoor ultraviolet radiation for 15 days, and a friction wheel made of rubber was arranged on the surface of the outdoor polyurethane simulated wood grain material, and rotated and rubbed with the material for 2 minutes at intervals of 30 minutes, so as to detect the yellowing ratio and mass loss of the outdoor polyurethane simulated wood grain material. At the same time, the surface water vapor resistance was tested according to the GB-17657 standard. Level 1: bubbling and / or delamination. Level 2: obvious changes in color and / or gloss. Level 3: moderate changes in color and / or gloss. Level 4: slight gloss and / or color changes can be seen when observed at a certain angle. Level 5: no changes.
[0078] Yellowing ratio = yellowing area / total exposed area of outdoor polyurethane simulated wood grain material.
[0079] Mass loss = mass of material before exposure - mass after the experiment.
[0080] The results are shown in the following table.
[0081]
[0082] It can be seen from the above table that the outdoor polyurethane simulated wood grain material prepared by the present invention has excellent weather resistance, excellent wear resistance, and a long outdoor service life.
[0083] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Changes, modifications, additions or substitutions made by ordinary technicians in this technical field within the essential scope of the present invention also fall within the protection scope of the present invention.
Claims
1. A polyurethane simulated wood grain material for outdoor use, which is composed of an outer layer, a decorative layer and a main body layer. Features: The outer layer is composed of two components, wherein component A includes: polyether polyol, diisocyanate, and hydrophilic chain extender, and component B includes: modified HDI trimer; wherein component A is prepared by mixing polyether polyol, diisocyanate, and hydrophilic chain extender and heating them for reaction; The modified HDI trimer is composed of HDI trimer, polytetrafluoroethylene, graphene oxide and polyetheretherketone, and is specifically prepared as follows: HDI trimer, polytetrafluoroethylene and polyetheretherketone are mixed in a ratio of 5:3:1 to form a mixture, and then aged at 35-40°C for 10-15min, and then 1 / 3 of the mass of the mixture of graphene oxide is added to the mixture, and the mixture is fully stirred and mixed to obtain the modified HDI trimer; The modification layer is composed of two components, wherein component A includes: polyol and diisocyanate, and component B includes the following components by weight: 100 parts of polyol, 0.5-5 parts of 1,4-butanediol, 0.1-0.3 parts of antioxidant, 0.3-1.0 parts of light stabilizer, 0.3-3.0 parts of surfactant and pigment; wherein component A is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 3.0-9.0%; The main layer is composed of three components, wherein component A includes: polyol and diisocyanate, component B includes the following components in parts by weight: 100 parts of polyol, 0.5-5 parts of 1,4-butanediol, 0.02-1 parts of water, 0.1-0.3 parts of antioxidant, 0.3-1.0 parts of light stabilizer, 0.3-3.0 parts of surfactant and pigment, 1-10 parts of inorganic filler, and component C includes the following components in parts by weight: 8-12 parts of reinforcing fiber, 1-3 parts of polyhydroxyacetic acid ester, 0.5-2.5 parts of nickel-1,2-dithiobenzothiadiazole coordination polymer; wherein component A is prepared by mixing and heating polyol and diisocyanate, and its NCO value is 3.0-11.0%.
2. The outdoor polyurethane simulated wood grain material according to claim 1, Features: The preparation process of the reinforcing fiber is as follows: firstly, glass fiber and modified aramid fiber are twisted in a ratio of 1:2 to form fiber twisted wire, then a cross-linking agent is sprayed on the surface of the fiber twisted wire, and the reinforcing fiber is obtained after drying.
3. The outdoor polyurethane simulated wood grain material according to claim 2, Features: The preparation process of the modified aramid fiber is as follows: the aramid fiber is hot-melted at 560-600°C to form an aramid fiber melt, and then nano-silicon oxide with a particle size of 10-20nm is added to the aramid fiber melt, and the ratio of the aramid fiber melt to the nano-silicon oxide is 3:
1. After mixing evenly, the aramid fiber melt is placed in a spinner, and extruded through the spinneret to form a melt stream with a diameter of 70-100nm, and then the melt stream is cooled to form a modified aramid fiber.
4. A method for preparing the outdoor polyurethane simulated wood grain material according to any one of claims 1 to 3, It is characterized in that The following steps are involved: S1. Making of silicone mold with wood grain: select wood with clear grain and suitable size, dry it, spray the release agent, and then pour room temperature vulcanized silicone rubber on the surface. After 24 hours of aging, demoulding can produce a silicone mold with wood grain on one side; S2. Preparation of the outer layer of polyurethane simulated wood grain material: placing the silicone mold in a mold frame and heating it, with the wood grain side facing upward, spraying a release agent on the surface, and then evenly mixing the AB components of the outer layer according to a certain proportion, and applying them to the grain surface of the silicone mold by spraying or brushing to obtain the outer layer of polyurethane simulated wood grain material; S3, preparation of polyurethane simulated wood grain material modification layer: after mixing the AB components of the modification layer evenly in proportion, apply them to the outer layer of the polyurethane simulated wood grain material by spraying or scraping to prepare the polyurethane simulated wood grain material modification layer; S4, preparation of the main layer of polyurethane simulated wood grain material: after the ABC components of the main layer are mixed evenly in proportion, they are applied on the polyurethane simulated wood grain material modification layer by spraying or scraping to prepare the main layer of polyurethane simulated wood grain material; S5. Demolding of finished product: After the maturation of each layer is completed, the product is removed from the silicone mold as a whole, so that the polyurethane simulated wood grain material can be obtained.
5. The method for preparing the outdoor polyurethane simulated wood grain material according to claim 4, Features: The wood in step S1 is made by weathered wood, carbonized wood or roughened wood.
6. The method for preparing the outdoor polyurethane simulated wood grain material according to claim 4, Features: In step S1, the room temperature vulcanized silicone rubber poured on the wood surface has a thickness of 3-10 mm.
Citation Information
Patent Citations
Environment-friendly anti-yellowing polyurethane composition
CN106008902A
Black-white-black three-layer shading film
CN115742519A
Preparation method of modified graphene polyurethane conductive film
CN117524581A
Laminate and manufacturing method of laminate
JP2007136993A
High weather resistant decorative sheet
JP2009113496A