A method for preparing aluminum-doped cerium oxide nanoabrasive
The preparation of aluminum-doped cerium oxide nanoabrasives solves the problem of insufficient Ce3+ and oxygen vacancy activity of rare earth cerium oxide abrasives in semiconductor polishing, improves polishing efficiency and process simplicity, is suitable for silicon dioxide polishing, and achieves high efficiency and high efficiency. Environmentally friendly polishing effect.
Patent Information
- Application Number
- CN202411045388.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The existing rare earth cerium oxide abrasives have low Ce3+ concentration and oxygen vacancy density during the semiconductor polishing process, resulting in low polishing efficiency, and the modification process is complex and difficult to scale up.
Using the preparation method of aluminum-doped cerium oxide nanoabrasives, ultrasonic dispersion of cerium salts, addition of aluminum precursors and strong alkali and weak acid salt solutions, magnetic stirring and calcination are performed to optimize the aluminum doping amount and oxygen vacancy activity to form a high Ce3+ content and nanoabrasives with high oxygen vacancy activity.
It improves the polishing removal rate and abrasion amount, simplifies the process route, achieves green and sustainable development, and is suitable for chemical mechanical polishing of silica.
Smart Images

Figure CN118562447B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of rare earth materials, in particular to a method for preparing aluminum-doped cerium oxide nano-abrasive. Background Art
[0002] As the size of electronic devices and their semiconductors in the integrated circuit industry becomes smaller and smaller, the performance requirements for semiconductors are getting higher and higher. As the semiconductor process nodes continue to shrink, the requirements for semiconductor surface flatness are also increasing. It is worth noting that chemical mechanical polishing (CMP) is the only process to achieve global flatness of integrated circuits. The most core consumables in the CMP process are polishing fluids, which account for as much as 49% of the cost. Rare earth cerium oxide (CeO2) is a key abrasive for polishing three-dimensional stacked flash memory (3D NAND) and shallow trench isolation (STI) structure devices used in key processes of integrated circuit chips due to its advantages such as high polishing rate, high chemical reaction activity, good selectivity and good surface finish.
[0003] At present, the modification of polishing abrasives in practical applications mainly consists of physical modification and surface grafting modification. It mainly prevents slurry agglomeration, stratification, and hardening to solve the problems of scratches and pitting on the workpiece. This method focuses on the process of using abrasives to make polishing liquid. Its modifiers are diverse, and the modification structure and process are becoming more and more complicated and cumbersome, which makes it difficult to mass produce, seriously restricting its large-scale application and promotion. At the same time, in the existing technology, due to the presence of CeO2 abrasives on the surface 3+ The low concentration content and oxygen vacancy density result in low efficiency of Ce-O-Si complexation during the polishing process, leading to low polishing efficiency.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The first purpose of the present invention is to provide a method for preparing aluminum-doped cerium oxide nanoabrasives. The preparation method has a simple route, is green and environmentally friendly, and conforms to the concept of sustainable development. At the same time, the preparation method can improve Ce 3+ The content and oxygen vacancy active centers are increased, so that the size of the finally prepared aluminum-doped cerium oxide nanoabrasive is high and the polishing removal rate is high.
[0006] The second object of the present invention is to provide the application of the preparation method of the above-mentioned aluminum-doped cerium oxide nanoabrasive in chemical mechanical polishing of silicon dioxide. When the abrasive is used to prepare a polishing liquid for mechanical polishing of SiO2, it has a higher polishing rate and polishing amount.
[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0008] The present invention provides a method for preparing an aluminum-doped cerium oxide nanoabrasive, comprising the following steps:
[0009] The cerium salt is ultrasonically dispersed in ionized water and subjected to an oil bath;
[0010] Then, an aluminum precursor is added and magnetic stirring is performed to obtain a mixed solution;
[0011] Slowly adding a strong base and weak acid salt solution to the mixed solution, followed by aging and separation to obtain a solid;
[0012] The solid is dried, ground and calcined to obtain;
[0013] The strong base and weak acid salt solution is a mixture of any one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, lactate or citrate solution;
[0014] The molar ratio of the cerium element in the cerium salt to the carbonate or bicarbonate contained in the strong base and weak acid salt solution = (1:0.5) - (1:5);
[0015] The temperature of the oil bath is 30°C-90°C.
[0016] In the present invention, the cerium salt dispersed in the ionized water is subjected to an oil bath. The temperature of the oil bath will directly affect the decomposition rate of the strong base weak acid salt and the generation of aluminum carbonate and cerium carbonate solid solution mixtures by the aluminum precursor in the reaction system. When the reaction temperature is low, not only will the reaction time be prolonged, but aluminum carbonate may also not be generated; when the reaction temperature is high, the strong base weak acid salt will be rapidly decomposed to generate aluminum hydroxide and cerium carbonate, and the required solid solution mixture cannot be generated. In the prior art, direct heating or water bath heating is generally used. When direct heating is used, it is difficult to ensure uniform heating; and when heating is performed by water bath heating, water is easily evaporated, affecting the reaction.
[0017] In the present invention, when selecting raw materials, a strong base weak acid salt solution that can produce weakly acidic release products is preferred, because the strong base weak acid salt solution will not affect the solid solution mixture of aluminum carbonate and cerium carbonate; and when the strong base weak acid salt solution is selected, not only can the co-precipitation of aluminum carbonate and cerium carbonate be ensured, but also unnecessary impurity ions can be removed during the subsequent calcination process.
[0018] The strong base and weak acid salts selected in the present invention are all soluble salt solutions because insoluble salts (such as calcium carbonate, etc.) contain CO3 2- , but it cannot decompose a large amount of CO3 2-Participate in the reaction. At the same time, the amount of cerium salt and strong base weak acid salt is limited in the present invention. In the present invention, the strong base weak acid salt not only reacts with the cerium salt, but also reacts with the aluminum precursor. In the present invention, the molar ratio of the cerium salt to the carbonate or bicarbonate contained in the strong base weak acid salt solution is preferably (1:0.5)-(1:5). Since the amount of aluminum doping affects the polishing rate of the prepared abrasive, the strong base weak acid salt solution added in the present invention not only reacts with the cerium salt, but also reacts with the aluminum precursor. Therefore, it is necessary to ensure that the cerium salt and the strong base weak acid salt are within a relatively reasonable ratio range to ensure that the cerium salt is completely reacted and no impurities are generated. When the cerium salt is obviously excessive, the cerium element cannot be completely precipitated as cerium carbonate; and when the strong base weak acid salt solution is obviously excessive, the generated carbonate and cerium carbonate will be mixed, resulting in the generation of impurities and affecting the performance of the abrasive.
[0019] Meanwhile, in the present invention, strong base and weak acid salt are selected as reaction raw materials, and wet chemical precipitation method is adopted to avoid the use of ammonia water or other raw materials that are easy to produce harmful gases, so that the process is simpler and more economical, and the physical properties of the prepared abrasive can be improved.
[0020] Preferably, as a further specific embodiment, one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate are added at the same time as lactate and / or citrate;
[0021] Preferably, the strong base and weak acid salt solution is a mixed salt solution of lactate and sodium bicarbonate;
[0022] Preferably, the molar ratio of the cerium element in the cerium salt to the bicarbonate in the strong base and weak acid salt solution is 1:2.
[0023] In the present invention, when carbonate or bicarbonate is selected alone, the hydrolysis ability of the aluminum salt precursor is reduced, and the calcination time is slightly increased. When lactate or citrate is selected alone, since the two salt solutions are organic salt solutions, and the organic salt solution has a hydrolysis equilibrium in the aqueous solution, the cerium salt cannot be completely precipitated. Since the effect of using any salt alone is not the best choice, a certain amount of carbonate or bicarbonate is added to lactate and / or citrate during actual use. This method of use can make the two organic functional groups of lactic acid or citric acid (obtained by hydrolysis of lactate or citrate) act as surfactants during the reaction process, thereby making the prepared abrasive particles more delicate; at the same time, the physical properties of the abrasive are improved.
[0024] Since the acidity of citric acid is slightly higher than that of lactic acid, and the alkalinity of citrate is slightly lower than that of lactate, the ability of lactate to adjust pH is slightly stronger than that of citrate; therefore, when citrate or lactate is selected as a mixed solution, lactate and sodium bicarbonate are more likely to be mixed. When a mixture of sodium bicarbonate and lactate is preferred, sodium bicarbonate will slowly decompose into sodium carbonate and carbon dioxide. The generated carbon dioxide can adjust the pH value of the solution and slowly regulate the hydrolysis equilibrium of the aluminum salt precursor. At the same time, the lactic acid produced by the hydrolysis of lactate can also adjust the pH and make the prepared abrasive smoother.
[0025] In the present invention, the molar ratio of the cerium element in the cerium salt to the bicarbonate in the strong base weak acid salt solution is preferably 1:2. The amount of salt solution used will affect the amount of cerium oxide nanoabrasive generated, resulting in changes in its polishing rate and polishing amount. When the preferred ratio is 1:2, the cerium salt can be completely reacted to increase the amount of nanoabrasive generated; at the same time, the polishing rate and polishing amount of the nanoabrasive can be improved.
[0026] Preferably, as a further specific embodiment, the magnetic stirring time is 2h-12h;
[0027] Preferably, as a further specific implementation manner, the magnetic stirring time is 2 hours.
[0028] Preferably, as a further specific implementation manner, the aging time is greater than or equal to 3 hours, and the drying time is greater than or equal to 6 hours.
[0029] Preferably, as a further specific embodiment, the cerium salt is a mixture of any one or more of cerium nitrate, cerium carbonate, cerium chloride, cerium octoate, ammonium cerium nitrate, ammonium cerium carbonate, ammonium cerium sulfate, cerium sulfide and cerium sulfate;
[0030] The aluminum precursor is a mixture of one or more of aluminum chloride, aluminum sulfate, alum, aluminum silicate, sodium aluminate, and aluminum sulfide.
[0031] Preferably, as a further specific implementation, the cerium salt is cerium nitrate; and the aluminum precursor is sodium aluminate.
[0032] When selecting a cerium salt, the selected cerium salt is a soluble cerium salt, which can be dissolved in the reaction system to generate two precipitates of aluminum carbonate and cerium carbonate, thereby increasing the polishing rate. In the present invention, the cerium salt is preferably cerium nitrate; the aluminum precursor is preferably sodium aluminate. Although other soluble cerium salts and aluminum precursors can participate in the reaction system, there may be a situation where the reaction is incomplete, and the reason is that there will be ions (such as chloride ions) that cannot be removed by calcination. In addition, in the present invention, a strong base and weak acid salt solution reacts with a cerium salt and an aluminum precursor to coprecipitate to generate cerium carbonate and aluminum carbonate, and the use of other aluminum precursors can certainly generate solid precipitates, but there can be no cerium carbonate and aluminum carbonate solid solutions. Although the polishing rate can also be improved, the effect is not as good as sodium aluminate and cerium nitrate.
[0033] Preferably, as a further specific embodiment, the molar ratio of the aluminum element in the aluminum precursor to the cerium element in the cerium salt is (1:100)-(50:100);
[0034] Preferably, the molar ratio of the aluminum element in the aluminum precursor to the cerium element in the cerium salt is (2:100)-(10:100).
[0035] In the present invention, the aluminum precursor used is also limited. When the aluminum content is high, although the appearance of the prepared metal abrasive is not much different during the reaction, aluminum oxide will be generated during the reaction. Aluminum oxide is relatively hard and will scratch the device, and the technical effect of the present invention cannot be achieved.
[0036] Preferably, as a further specific embodiment, the calcination temperature is 400°C-1000°C.
[0037] The calcination temperature determines the growth of the crystal form in the prepared nano-abrasive. High temperature can promote the change of the crystal form, make the particles of the nano-abrasive more uniform, and improve its polishing rate.
[0038] The invention also provides an application of a preparation method of aluminum-doped cerium oxide nano-abrasive in chemical mechanical polishing of silicon dioxide.
[0039] In the present invention, the prepared nanoabrasive is cerium oxide particles with uniform size. The prepared cerium oxide is used to prepare a polishing liquid. The main components of the polishing liquid are: cerium oxide solution, dispersant and pH adjuster (CA and TEAH), and the solid content of the polishing liquid is within the range of 5%-10%, which can significantly improve the removal rate and the amount of polishing. When the solid content is 7.5%, the performance of the prepared polishing liquid is the best.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] The nano-abrasive prepared by the preparation method has high Ce 3+ The content and rich oxygen vacancy activity, uniform size and high polishing removal rate, high polishing rate and high polishing amount; the preparation process of the invention is simple, green and environmentally friendly, and in line with the concept of sustainable development. The nano-abrasive Ce prepared by the preparation method of the invention 3+ The content is as high as 27.96%. The polishing liquid prepared with this abrasive has a polishing rate of up to 0.2302 mg / min and an erosion amount of 1.0542 g. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 : Al in Example 1 0.1 @SEM image of CeO2(600) nanoabrasive;
[0043] Figure 2 : Al in Example 4 0.1 @SEM image of CeO2(1000) nanoabrasive;
[0044] Figure 3 : XDR images of cerium oxide abrasives at different temperatures and different aluminum content;
[0045] Figure 4 :Al 0.1 @TEM image of CeO2(1000) nanoparticles. DETAILED DESCRIPTION
[0046] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0047] Example 1
[0048] Preparation of polishing powder.
[0049] Add 43.42g Ce(NO3)3•6H2O to 50mL deionized water and transfer to a 250mL round-bottom flask heated in an oil bath. When the temperature of the oil bath rises to 30°C, use a peristaltic pump to drip 50mL of sodium aluminate aqueous solution (0.1mol / L) into the above flask at a flow rate of 1mL / min. After magnetic stirring in an oil bath at 65°C for 2h, a mixed solution is obtained. A certain concentration of sodium bicarbonate mixed salt solution (8.4 g / 100 mL) is slowly added to the above mixed solution and aged for 3h. After centrifugation, washing, drying in a 120°C oven for 6h and grinding, the obtained yellow solid is transferred to a 600 °C muffle furnace and calcined for 5h. Get Al 0.1 @CeO 2 (600)(Al x @CeO 2 (y)) Sample (e.g. Figure 1 For simplicity of description, x and y are the sodium aluminate concentration and the calcination temperature, respectively.
[0050] Polishing experiment
[0051] The polishing experiment was carried out using the UNIPOL-1200S automatic pressure grinding and polishing machine produced by Shenyang Kejingzi Company, and the polishing pad model was IC1010 (purchased from Dow Electronic Materials, USA). The polishing process parameters are as follows: the fixed polishing pressure is 6.0 kg (1 kg = 0.1MPa), the polishing head and the polishing disc speed are 87r / min and 93r / min respectively, the polishing liquid flow rate is 300mL / min, and the polishing time is 1min. The composition of the polishing liquid: cerium oxide solution (solid content 7.5%), dispersant, pH adjuster (CA and TEAH). The thickness before and after polishing was measured using a spiral micrometer. During the test, 30 points were taken from the front to the back on the central symmetry line of the wafer, and the thickness values were recorded. The removal rate and the polishing amount were calculated by the formula (MRR = Δh / t) and the weight difference, respectively.
[0052] Example 2
[0053] The specific implementation steps are consistent with those in Example 1, except that only the molar ratio of aluminum to cerium is changed.
[0054] When the molar ratio is 0.5:100, the concentration of sodium aluminate is 0.01 mol / L, and Al 0.01 @CeO2(600) nanoabrasive;
[0055] When the molar ratio is 1:100, the concentration of sodium aluminate is 0.02 mol / L, and Al 0.02 @CeO2(600) nanoabrasive;
[0056] When the molar ratio is 5:100, the concentration of sodium aluminate is 0.1 mol / L, and Al 0.1 @CeO2(600) nanoabrasive;
[0057] When the molar ratio is 10:100, the concentration of sodium aluminate is 0.2 mol / L, and Al 0.2 @CeO2(600) nanoabrasive;
[0058] When the molar ratio is 15:100, the concentration of sodium aluminate is 0.3 mol / L, and Al 0.3 @CeO2(600) nano abrasive;
[0059] When the molar ratio is 25:100, the concentration of sodium aluminate is 0.5 mol / L, and Al 0.5 @CeO2(600) nano abrasive;
[0060] When the molar ratio is 50:100, the concentration of sodium aluminate is 1 mol / L, and the nano-abrasive Al1@CeO2(600) is prepared;
[0061] When the molar ratio is 60:100, the concentration of sodium aluminate is 1.2 mol / L, and Al 1.2 @CeO2(600) nanoabrasive;
[0062] The prepared cerium oxide nanoabrasive was prepared into a polishing liquid for mechanical polishing. The removal rate and polishing amount were measured using the polishing experiment in Example 1. The experimental results are shown in Table 1.
[0063] Table 1: Effect of different Al doping amounts on the Ce content of cerium oxide nanoabrasives 3+ The influence of content and its polishing rate and polishing amount;
[0064] .
[0065] It can be seen from the experimental data of Example 2 that the polishing performance of aluminum-doped cerium oxide nanoabrasive is higher than that of pure cerium oxide nanoabrasive. Different doping amounts have an important influence on the polishing performance of cerium oxide nanoabrasive. When the aluminum content is within a suitable range, the oxygen vacancy sites increase, which is more conducive to the polishing of silicon oxide. When the aluminum content is excessive, aluminum oxide with greater hardness is generated during the reaction, and aluminum oxide can cause the polishing liquid to scratch the device, resulting in a decrease in its various physical properties; and when the aluminum content is low, the number of aluminum atoms occupying the cerium oxide lattice is small, resulting in Ce on the surface of the cerium oxide. 3+ The content is low, which affects its polishing performance.
[0066] Example 3
[0067] The specific implementation method is the same as Example 1, except that the molar ratio of sodium bicarbonate to cerium nitrate is changed.
[0068] When the molar ratio of the cerium element in cerium nitrate to the bicarbonate in sodium bicarbonate is 0.5:1, the mass of the sodium bicarbonate used is 2.1 g;
[0069] When the molar ratio of the cerium element in cerium nitrate to the bicarbonate in sodium bicarbonate is 1:0.5, the mass of the sodium bicarbonate used is 4.2 g;
[0070] When the molar ratio of the cerium element in cerium nitrate to the bicarbonate in sodium bicarbonate is 1:1, the mass of the sodium bicarbonate used is 8.4 g;
[0071] When the molar ratio of the cerium element in cerium nitrate to the bicarbonate in sodium bicarbonate is 1:2, the mass of the sodium bicarbonate used is 16.8 g;
[0072] When the molar ratio of the cerium element in cerium nitrate to the bicarbonate in sodium bicarbonate is 1:5, the mass of the sodium bicarbonate used is 42 g;
[0073] When the molar ratio of the cerium element in cerium nitrate to the bicarbonate in sodium bicarbonate is 1:7, the mass of the sodium bicarbonate used is 58.8 g;
[0074] The removal rate and polishing amount were determined using the polishing experiment in Example 1. The experimental results are shown in Table 2.
[0075] Table 2: Effect of different molar ratios of cerium salts to sodium bicarbonate on the Ce content of cerium oxide nanoabrasives 3+ The influence of content and its polishing rate and polishing amount,
[0076] .
[0077] It can be seen from the experimental data of Example 3 that the change of the mass of sodium bicarbonate will not affect the surface of the cerium oxide nanoabrasive Ce 3+ content, but the polishing rate and the amount of polishing will change with the change of the amount of sodium bicarbonate. When the selected amount of sodium bicarbonate added is within the range selected by the present invention, the polishing rate and the amount of polishing will increase with the increase of sodium bicarbonate. The reason is that the amount of sodium bicarbonate affects the amount of cerium oxide nanoabrasive generated, resulting in changes in its polishing rate and amount of polishing. When the sodium bicarbonate content is excessive, its solubility is reduced, and the carbonate itself will precipitate, causing the solid carbonate and cerium carbonate to solidify, making it impossible to separate the abrasive, and the prepared abrasive contains more impurities; and when the sodium bicarbonate content is low, the aluminum element and the cerium salt in the reaction system cannot be fully precipitated, thereby affecting its physical properties.
[0078] Example 4
[0079] The specific implementation is the same as that of Example 1, except that only the calcination temperature is changed.
[0080] When the calcination temperature is 200°C, Al 0.1 @CeO2(200);
[0081] When the calcination temperature is 400 °C, Al 0.1 @CeO2(400);
[0082] When the calcination temperature is 600 °C, Al 0.1 @CeO2(600);
[0083] When the calcination temperature is 800 °C, Al 0.1 @CeO2(800);
[0084] When the calcination temperature is 1000 °C, Al 0.1 @CeO2(1000);
[0085] When the calcination temperature is 1200 °C, Al 0.1 @CeO2(1200);
[0086] The polishing experiment in Example 1 was used to determine the removal rate and polishing amount. The experimental results are shown in Table 3, where Al 0.1 @CeO2(1000) SEM picture Figure 2 shown.
[0087] Table 3: Effect of different calcination temperatures on the Ce content of aluminum-doped cerium oxide nanoabrasives 3+ The influence of content and its polishing rate and polishing amount;
[0088]
[0089] The experimental results of Example 4 show that different calcination temperatures have an important influence on the polishing performance of aluminum-doped cerium oxide nanoabrasives. Higher calcination temperatures are conducive to the formation of oxygen vacancies and Ce 3+ The content increases, thereby increasing the removal rate and the amount of polishing; although the above-mentioned abrasive can also be obtained at low temperatures, low temperatures may cause the calcination time to become longer and are not conducive to the formation of oxygen vacancies, thereby reducing the performance of the prepared abrasive in various aspects.
[0090] Al 0.1 @CeO2(600) and Al 0.1 @CeO2(1000) SEM image of nanoabrasive ( Figure 1 and Figure 2 ) were compared, and the results showed that Al 0.1 @CeO2(600) Nano-abrasive is composed of fine CeO2 primary nano-particles and maintains a certain uniform dispersion. And the primary nano-particles tend to aggregate to form secondary particles. When the temperature increases to 1000 ℃, Al 0.1 @CeO2(1000) nanoparticles show a geometric growth of large particles and a tendency to further agglomerate. It can be seen that 600℃ is the most suitable calcination temperature.
[0091] Figure 3 The XDR images of cerium oxide abrasives at different temperatures and different aluminum content are shown. The spectra show that the strong XRD peaks of CeO2 phase appear at 28.6°, 33.1°, 47.5°, 56.3°, 59.1°, 69.4°, 76.7° and 79.1°, corresponding to the (1 1 1), (2 0 0), (2 2 0), (3 1 1), (2 2 2), (4 0 0), (3 31), (4 4 0) and (4 2 0) crystal planes of CeO2 (JCPDS 34-0394), respectively. In addition to the characteristic peaks of CeO2 phase, no obvious characteristic peaks of Al2O3 and CeAl compounds are observed; the reason is that the metal Al2O3 component can be well dispersed in CeO2. Figure 4 The results show that Al@CeO2 abrasives are successfully synthesized and Al doping does not change the crystalline structure of CeO2 particles. Figure 4 Proof, Al 0.1 @In the TEM image of CeO2(1000) nanoparticles, a lattice fringes of 0.504 nm was found, which was attributed to the (0 5 11) crystal plane of Al2O3 phase (JCPDS 46-1131). Figure 4 It proves that Al is successfully doped into CeO2 abrasive.
[0092] Example 5
[0093] The specific implementation method is the same as that of Example 1, except that only the temperature of the oil bath is changed. The temperatures of the oil bath are set to 20°C, 30°C, 60°C, 90°C, and 105°C, respectively, and the polishing experiment in Example 1 is used to measure the removal rate and polishing amount. The experimental results are shown in Table 4.
[0094] Table 4: Effect of different oil bath temperatures on Al 0.1 @CeO2(600)Nano-abrasive Ce 3+ The influence of content and its polishing rate and polishing amount;
[0095] .
[0096] It can be seen from the experimental results of Example 5 that different oil bath temperatures have an important influence on the polishing performance of aluminum-doped cerium oxide nanoabrasives. Under the experimental conditions, the temperature of the oil bath affects the formation of aluminum carbonate, which is beneficial to the formation of cerium oxide nanoabrasives; when the temperature is low or at room temperature, the reaction is slow and almost no aluminum carbonate is generated; when the temperature is high, the rapid decomposition of bicarbonate leads to the formation of aluminum hydroxide, which makes the Ce of the abrasive 3+ The content, polishing rate and erosion amount are reduced.
[0097] Example 6
[0098] The specific implementation steps are consistent with Example 1, only the reaction conditions are changed.
[0099] The magnetic stirring time was set to 2 h and 12 h respectively;
[0100] Set the aging time to 3h or 5h;
[0101] Set the drying time to 6h or 10h.
[0102] The polishing experiment in Example 1 was used to determine the removal rate and the amount of polishing. The experimental results are shown in Table 5.
[0103] Table 5: Effect of different reaction conditions on Al 0.1 @CeO2(600)Nano-abrasive Ce 3+ The influence of content and its polishing rate and polishing amount,
[0104] .
[0105] It can be seen from the experimental results of Example 6 that different reaction conditions have a great influence on the performance of the cerium oxide nanoabrasive. Preferably, under the reaction conditions selected by the present invention, the reaction can be completed; at the same time, the impurities generated during the reaction process are reduced, thereby improving the performance of the abrasive.
[0106] Example 7
[0107] Specific implementation method As in Example 1, a mixture of sodium bicarbonate and sodium lactate (hereinafter referred to as mixed solution 1) is used to react with cerium nitrate.
[0108] Scheme 1: The molar ratio of cerium element in cerium nitrate to bicarbonate in mixed solution 1 is 1:0.5;
[0109] Scheme 2: The molar ratio of cerium element in cerium nitrate to bicarbonate in mixed solution 1 is 1:2;
[0110] Scheme 3: The molar ratio of the cerium element in cerium nitrate to the bicarbonate in mixed solution 1 is 1:5;
[0111] Scheme 4: The molar ratio of the cerium element in cerium nitrate to the bicarbonate in mixed solution 1 is 0.5:1;
[0112] Scheme 5: The molar ratio of the cerium element in cerium nitrate to the bicarbonate ion in the mixed solution 1 is 1:7.
[0113] The removal rate and polishing amount were determined using the polishing experiment in Example 1. The experimental results are shown in Table 6.
[0114] Table 6: Effect of different molar ratios of sodium bicarbonate and sodium lactate on Al 0.1 @CeO2(600)Nano-abrasive Ce 3+ The influence of content and its polishing rate and polishing amount,
[0115] .
[0116] From the above experimental results, it can be seen that after mixing sodium bicarbonate and sodium lactate for reaction, Ce 3+ The content and polishing rate are not affected, and the polishing amount and output at certain ratios will be slightly reduced. Since sodium lactate can participate in the reaction as a surfactant, the produced nano-abrasive particles can be made smaller and finer, which can better solve the technical problem proposed by the present invention.
[0117] Comparative Example 1
[0118] When an insoluble carbonate is used for the reaction, the reaction cannot proceed and the abrasive cannot be prepared.
[0119] Comparative Example 2
[0120] The molar ratio of the cerium salt to the strong base and weak acid salt solution was changed, and the removal rate and the polishing amount were measured using the polishing experiment in Example 1. The experimental results are shown in Table 7.
[0121] Table 7: Changes in the molar ratio of cerium nitrate to sodium bicarbonate for Ce of nanoabrasives 3+ The influence of content and its polishing rate and polishing amount,
[0122] .
[0123] By comparing the experimental results of Example 3 with those of Comparative Example 2, it can be seen that when the amount of cerium nitrate is obviously excessive, it cannot be completely precipitated as cerium carbonate. In the subsequent calcination, the cerium nitrate decomposes into nitrogen oxide gas and cerium oxide. The gas is harmful to the environment. At the same time, the effective Ce in the prepared nanoabrasive 3+ The content is reduced, resulting in a decrease in removal rate and erosion amount; when sodium bicarbonate is excessive, it will directly lead to the generation of impurities containing carbonate and cannot be separated from the intermediate product cerium carbonate. After calcination, the nano abrasive becomes uneven and various physical properties are reduced.
[0124] Comparative Example 3
[0125] Cerium carbonate was used as the raw material, water-soluble aluminum salt and excess ammonia water were added, mechanically ball-milled, then dried and redispersed, calcined at high temperature, and ball-milled after cooling. The removal rate and polishing amount were determined using the polishing experiment in Example 1. The experimental results are shown in Table 8.
[0126] Table 8: Effects of different reaction methods on Ce of nanoabrasives 3+ The influence of content and its polishing rate and polishing amount,
[0127] .
[0128] Al in Example 2 0.3 @CeO2(600) is the optimal reaction result in the present invention, so this group of experimental data is compared with Comparative Example 3.
[0129] By comparing the experimental data of Example 3 with that of Example 2, it can be seen that in the present invention, since the use of ammonia water is avoided, no waste gas is generated in the reaction, and the atomic utilization rate is higher, so the Ce 3+ The content is higher, so that the physical properties of the prepared abrasive are significantly improved. However, the reaction method of Comparative Example 3 has more intermediate products, which leads to lower atomic utilization, and ultimately lower physical properties of the obtained nano abrasive.
[0130] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing aluminum-doped cerium oxide nanoabrasive, characterized in that: The steps include: The cerium salt is ultrasonically dispersed in ionized water and subjected to an oil bath; Then, an aluminum precursor is added and magnetic stirring is performed to obtain a mixed solution; Slowly adding a strong base and weak acid salt solution to the mixed solution, followed by aging and separation to obtain a solid; The solid is dried, ground and calcined to obtain; The strong base and weak acid salt solution is a mixture of any one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, lactate or citrate solution; While adding lactate and / or citrate, one or more of sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate are added; The molar ratio of the cerium element in the cerium salt to the carbonate or bicarbonate contained in the strong base and weak acid salt solution = (1:0.5) - (1:5); The temperature of the oil bath is 30°C-90°C; The cerium salt is a mixture of any one or more of cerium nitrate or ammonium cerium nitrate; The aluminum precursor is a mixture of one or more of aluminum chloride, aluminum sulfate, alum, aluminum silicate, sodium metaaluminate, and aluminum sulfide; The molar ratio of the aluminum element in the aluminum precursor to the cerium element in the cerium salt is (1:100)-(50:100); Calcination temperature is 400°C -1000°C; The molar ratio of the cerium element in the cerium salt to the bicarbonate in the mixed salt solution of lactate and sodium bicarbonate is 1:
2.
2. The method for preparing aluminum-doped cerium oxide nanoabrasive according to claim 1, characterized in that: The magnetic stirring time is 2h-12h.
3. The method for preparing the aluminum-doped cerium oxide nanoabrasive according to claim 2, characterized in that: The magnetic stirring time is 2h.
4. The method for preparing aluminum-doped cerium oxide nanoabrasive according to claim 1, characterized in that: The aging time is greater than or equal to 3 hours, and the drying time is greater than or equal to 6 hours.
5. The method for preparing aluminum-doped cerium oxide nanoabrasive according to claim 1, characterized in that: The cerium salt is cerium nitrate; The aluminum precursor is sodium aluminate.
6. Application of the preparation method of aluminum-doped cerium oxide nanoabrasive according to any one of claims 1 to 5 in chemical mechanical polishing of silicon dioxide.
Citation Information
Patent Citations
Aluminum doped cerium rouge and preparation method thereof
CN101696345A
Preparation method for cerium oxide and application of cerium oxide to STI chemico-mechanical polishing
CN106915761A
Nanocrystal-containing cerium oxide flaky powder and preparation method thereof
CN118359222A
Chemical-mechanical polishing slurry composition and method for manufacturing semiconductor by using the same
KR102373919B1
Methods of controlling the properties of abrasive particles for use in chemical-mechanical polishing slurries
US20060032836A1