Extruder barrel wear-resistant alloy coating, laser cladding method and cladding gun head

By using wear-resistant alloy coatings prepared by using nickel-chromium matrix powder and hard ceramic particles on the inner wall of the extruder barrel, combined with laser cladding technology, the problems of wear and difficulty in assembly of the barrel wall and alloy bushing are solved, and the problem of high difficulty in assembly of the alloy bushing is achieved. Efficient and low-cost wear resistance and extended service life.

CN118563313BActive Publication Date: 2024-11-12ACUNITY TIANJIN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411036427.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

During use, the inner wall corrosion and wear of hard materials caused by wear of the existing extruder barrels. The traditional built-in alloy set is difficult to fit, has high cost and insufficient wear resistance, which cannot effectively extend the service life.

Method used

Wear-resistant alloy coatings are prepared using nickel-chromium matrix powder and hard ceramic particles. Wear-resistant alloy coatings and non-wear-resistant alloy coatings are formed on the half side of the inner wall of the barrel through laser cladding technology, and dual-channel powder feeding channels and lasers are used. The cladding spear tip achieves efficient cladding, combining rotation and laser irradiation to form an integrated coating.

Benefits of technology

The maximum utilization of materials is achieved, the cost is reduced, the wear resistance of the inner wall of the barrel is significantly improved, the service life is extended, and the problems of mechanical fit and poor thermal conductivity of traditional alloy bushings are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118563313B_ABST
    Figure CN118563313B_ABST
Patent Text Reader

Abstract

The present invention relates to a wear-resistant alloy coating for an extruder barrel, a laser cladding method and a cladding gun head, wherein a wear-resistant alloy coating is clad on half of the inner wall of the extruder barrel, and a non-wear-resistant alloy coating is clad on the other half, wherein the wear-resistant alloy coating comprises nickel-chromium matrix powder and hard ceramic particles, the nickel-chromium matrix powder comprises NiCr35 and Ti powder, and the hard ceramic particles comprise W powder and C powder; at the same time, the cladding gun head comprises a gun head body, two nozzles at one end of the gun head body, a laser light source in the gun head body, a parabolic focusing copper mirror arranged at the end of the gun head body, and a powder feeding channel connected to the two nozzles, and each nozzle is respectively connected to two powder feeding channels. The process design of the present invention is scientific and reasonable, convenient, efficient and easy to implement, and effectively controls costs while ensuring maximum utilization of materials. At the same time, the wear resistance of the wear-resistant alloy coating disclosed in the present invention is much higher than that of the embedded alloy bushing, which effectively prolongs the service life and has a high application and promotion value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of laser cladding, and in particular to a wear-resistant alloy coating for an extruder barrel, a laser cladding method and a cladding gun head. Background Art

[0002] The barrel of a twin-screw extruder is the core component of a twin-screw extruder, and is mainly used to process PVC plastics and extrude plastic products such as tubes, plates, sheets, rods, films, and profiles. During the service of the extruder barrel, plastic base particles, auxiliary materials, and additives are mixed and kneaded in the barrel, especially hard materials such as calcium carbonate and glass fiber, which have a greater impact on the wear of the inner wall, causing the inner wall of the barrel to be severely corroded and worn and fail, so the barrel accessories have to be replaced. Therefore, it is particularly important to improve the performance of the extruder barrel, especially the wear resistance and corrosion resistance of the inner wall.

[0003] At the same time, during the service of the barrel, the screw will float up due to the "support" of the auxiliary materials below, resulting in serious wear on the upper inner wall of the barrel and almost no wear on the lower inner wall. The existing traditional process is to embed SKT11 alloy sleeves on the entire inner wall of the barrel. The main limitations are: first, the embedded alloy sleeves are difficult to assemble and the labor cost is high; second, the alloy sleeves and the barrel mechanically cooperate, and the thermal conductivity is poor, which affects the temperature control of the processed materials; third, it is impossible to prepare only half of the required wear-resistant alloys, the cost is very high, and it causes waste.

[0004] In summary, designing a laser cladding method for extruder barrel alloy coating with convenient cladding process and effective cost control while ensuring maximum material utilization has become a technical problem and research and development direction that needs to be urgently solved by technical personnel in this field. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies in the prior art and provide a wear-resistant alloy coating for an extruder barrel, a laser cladding method and a cladding gun head.

[0006] The present invention is achieved through the following technical solutions:

[0007] A wear-resistant alloy coating for an extruder barrel comprises nickel-chromium matrix powder and hard ceramic particles, wherein the nickel-chromium matrix powder comprises NiCr35 and Ti powder, and the hard ceramic particles comprise W powder and C powder, wherein the molar ratio of the Ti powder, W powder and C powder is 1:1:2.

[0008] According to the above technical solution, preferably, the NiCr35 includes the following chemical components: C 0.5-0.6%, B 2.5-3.0%, Si 3.5-4.0%, Cr 13-14%, Fe 4.5-5.5%, Ni BAL.

[0009] According to the above technical solution, preferably, the powder particle size of the NiCr35 is 50-105um, and the powder particle sizes of the Ti powder, W powder and C powder are 30-105um.

[0010] At the same time, this patent also discloses a laser cladding method for an extruder barrel. Based on the above-mentioned wear-resistant alloy coating of the extruder barrel, the wear-resistant alloy coating is clad on half of the inner wall of the extruder barrel, and the non-wear-resistant alloy coating is clad on the other half. Specifically, the following steps are included:

[0011] S1. placing the cladding gun head at the center of the extruder barrel and moving the cladding gun head horizontally to the starting cladding position;

[0012] S2. The upper and lower sides of the cladding gun head are respectively fed to the molten pool. Specifically, one side of the cladding gun head is fed with nickel-chromium matrix powder and hard ceramic particles, and the other side of the cladding gun head is fed with Fe35 powder;

[0013] S3. The extruder barrel rotates in a preset direction and angle so that half of the inner wall of the extruder barrel is coated with a wear-resistant alloy coating and the other half is coated with a non-wear-resistant alloy coating.

[0014] According to the above technical solution, preferably, the non-wear-resistant alloy coating is Fe35 powder, comprising the following chemical components: C 0.31%, B 1.11%, Si 1.22%, Cr 17.6%, Ni 2.21%, Mn 0.20%, Fe BAL.

[0015] According to the above technical solution, preferably, in step S2, the NiCr35 and Ti powders are ball-milled for 1 hour using a planetary ball mill, and nickel-chromium matrix powder is obtained after being evenly mixed; the nickel-chromium matrix powder and hard ceramic particles are then loaded into a V-type mixer and mixed for 30 minutes; and the powder is then delivered to the molten pool through the cladding gun head.

[0016] According to the above technical solution, preferably, in step S2, one side of the cladding gun head includes two powder feeding channels, and different powder-carrying airflows are used to transport the nickel-chromium matrix powder and hard ceramic particles to the molten pool.

[0017] In addition, this patent also discloses a cladding gun head, which is used for the laser cladding method of the above-mentioned extruder barrel, including a gun head body, two nozzles arranged opposite to each other on both sides of one end of the gun head body, a laser light source located in the middle of the gun head body, a parabolic focusing copper mirror arranged at the end of the gun head body relative to the laser light source, and powder feeding channels respectively connected to the two nozzles. Each of the nozzles is respectively connected to two powder feeding channels, and the parabolic focusing copper mirror can make the laser light emitted by the laser light source be emitted from the middle of the two nozzles respectively. At the same time, a protective gas channel and a cooling water channel are also provided on the gun head body.

[0018] The beneficial effects of the present invention are:

[0019] The process design of the present invention is scientific and reasonable, convenient, efficient and easy to implement. In the actual laser cladding process, the actual workpiece only needs to be rotated 180 degrees to complete the half-side cladding of the wear-resistant alloy coating and the half-side cladding of the non-wear-resistant alloy coating on the inner wall of the extruder barrel at one time, so as to maximize the utilization of materials and effectively control costs.

[0020] Compared with the traditional embedded alloy bushing, the alloy coating is metallurgically combined with the barrel to form an integral whole. At the same time, the wear resistance of the wear-resistant alloy coating disclosed in the present invention is much higher than that of the embedded alloy bushing, which effectively prolongs the service life and has a high application and promotion value. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a scanning electron microscope image of the wear-resistant alloy coating of the present invention.

[0022] Figure 2 It is a scanning electron microscope image of the non-wear-resistant alloy coating of the present invention.

[0023] Figure 3 These are the laser cladding processing parameters in Example 2 of the present invention.

[0024] Figure 4 The three-dimensional structure of Example 3 of the present invention is shown in FIG. Figure 1 .

[0025] Figure 5 The three-dimensional structure of Example 3 of the present invention is shown in FIG. Figure 2 .

[0026] Figure 6 The internal structure of the third embodiment of the present invention is three-dimensional Figure 1 .

[0027] Figure 7 The internal structure of the third embodiment of the present invention is three-dimensional Figure 2 .

[0028] Figure 8 It is a cross-sectional view of the main structure of Example 3 of the present invention.

[0029] In the figure: 1. Gun head body; 2. Nozzle; 3. Powder delivery channel; 4. Protective gas channel; 5. Cooling water channel; 6. Parabolic focusing copper mirror; 7. Beam splitter prism; 8. Laser light source. DETAILED DESCRIPTION

[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiment. Based on the embodiments in the invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the invention.

[0031] In the description of the invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" etc. indicating directions or positional relationships are based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they cannot be understood as limitations on the invention.

[0032] In addition, it should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "installation", "setting", and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, an indirect connection through an intermediate medium, or the internal connection of two components. For those skilled in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0033] Embodiment 1: A wear-resistant alloy coating for an extruder barrel, comprising a nickel-chromium matrix powder and hard ceramic particles, wherein the nickel-chromium matrix powder comprises NiCr35 and Ti powder (purity 99%), and the hard ceramic particles comprise W powder (purity 99.95%) and C powder (graphite, purity 99.5%), wherein the molar ratio of the Ti powder, W powder and C powder is 1:1:2. The NiCr35 comprises the following chemical components: C 0.5-0.6%, B 2.5-3.0%, Si 3.5-4.0%, Cr 13-14%, Fe 4.5-5.5%, NiBAL. Specifically, the powder particle size of the NiCr35 is 50-105um, and the powder particle size of the Ti powder, W powder and C powder is 30-105um. In this example, it is preferred but not limited to that the particle size of the Ti powder is 75um, the particle size of the tungsten powder (W powder) is 30um, and the particle size of the graphite (C powder) is 75um.

[0034] The wear-resistant alloy powder composed of nickel-chromium matrix powder and hard ceramic particles undergoes a chemical metallurgical reaction after melting and solidification, producing a series of densely dispersed fine hard phases in the matrix, which effectively increases the hardness of the coating matrix. At the same time, combined with large particles of additional tungsten carbide spherical particles, a high-hardness tungsten carbide reinforced wear-resistant coating is achieved.

[0035] When Ti, W and C exist in the molten pool at the same time, a chemical reaction will occur. Through Gibbs free energy calculation, it is found that the Gibbs free energy of the reaction between Ti and C is the lowest, and the Gibbs free energy of the reaction is less than zero, indicating that the reaction can proceed spontaneously. The C element will preferentially react with the Ti element to form a Ti / C hard ceramic phase. After Ti / C is generated, the free W will diffuse into the Ti / C lattice, occupy part of the Ti position, and form a (Ti, W) C solid solution. In addition, the C powder and W powder in the raw material also react in situ through laser cladding to generate WC ceramic particles (hard ceramic particles), W2C reinforcement phase W+C=WC, 2W+C=W2C, and at the same time, a large amount of Ni in NiCr35 combines with Fe, C, B and other elements to form Fe x C Iron-carbon compounds, (Fe, Ni) 23 C 26 Solid solutions such as Ni4B have a solid solution strengthening effect on the coating.

[0036] Figure 1 It is a wear-resistant alloy coating. Compared with non-wear-resistant alloy coating ( Figure 2 ), the matrix of the wear-resistant coating has significantly improved hardness and wear resistance due to the generation and dispersion of fine reinforcements, and the formed coating is: hard matrix + hard particle effect, achieving the effect of "strong combination". The conventional coating is: soft matrix + hard particle effect. During the use of this coating, due to the effect of abrasive wear, the soft nickel-based matrix on the surface is first and quickly worn away, the surface roughness of the coating increases sharply, the smoothness decreases, and the friction coefficient increases, resulting in serious damage to the friction pair (the friction pair in this working condition is the screw), causing damage to the equipment. The hard matrix + hard particle coating effect effectively avoids this problem.

[0037] Example 2: This patent also discloses a laser cladding method for an extruder barrel. Based on the above-mentioned wear-resistant alloy coating of the extruder barrel, a wear-resistant alloy coating is clad on half of the inner wall of the extruder barrel, and a non-wear-resistant alloy coating is clad on the other half, wherein the non-wear-resistant alloy coating is Fe35 powder, comprising the following chemical components: C 0.31%, B 1.11%, Si 1.22%, Cr17.6%, Ni 2.21%, Mn 0.20%, Fe BAL.

[0038] Laser cladding processing parameters such as Figure 3 As shown, the specific steps include:

[0039] S1. placing the cladding gun head at the center of the extruder barrel and moving the cladding gun head horizontally to the starting cladding position;

[0040] S2. The upper and lower sides of the cladding gun head are respectively fed to the molten pool. Specifically, one side of the cladding gun head is fed with nickel-chromium matrix powder and hard ceramic particles, and the other side of the cladding gun head is fed with Fe35 powder;

[0041] S3. The extruder barrel rotates in a preset direction and angle so that half of the inner wall of the extruder barrel is coated with a wear-resistant alloy coating and the other half is coated with a non-wear-resistant alloy coating.

[0042] It should be noted that, in step S2, the nickel-chromium matrix powder and hard ceramic particles are preferably delivered on one side of the cladding gun head in the following two ways, but not limited to:

[0043] First, the NiCr35 and Ti powders are ball-milled for 1 hour using a planetary ball mill, and nickel-chromium matrix powder is obtained after being evenly mixed; the nickel-chromium matrix powder and hard ceramic particles are then loaded into a V-type mixer and mixed for 30 minutes; and the powder is then delivered to the molten pool through the cladding gun head.

[0044] Secondly, one side of the cladding gun head includes two powder feeding channels, which use different powder-carrying airflows to transport the nickel-chromium matrix powder and hard ceramic particles to the molten pool. For the preparation of wear-resistant coatings, it is necessary to transport the nickel-chromium matrix powder and hard ceramic (such as WC) particles into the molten pool. Currently, the two powders are mechanically mixed and then fed into the molten pool through a powder feeding channel. However, due to the great difference in the physical density of the two powders (the density of the nickel-chromium matrix powder is about 7.2g / cm 3 , while the density of WC particles is about 15.6 g / cm 3 ), the tungsten carbide with higher density will sink to the bottom of the coating, resulting in obvious stratification problems in the prepared wear-resistant coating, and the surface content of tungsten carbide particles is very low. In order to avoid this problem, two powder feeding channels are designed in this scheme to transport nickel-chromium matrix powder and hard ceramic particles (WC particle powder) respectively. Each powder feeding channel uses a different powder-carrying airflow. The hard ceramic particles (WC particles) use a smaller powder-carrying airflow, so that the hard ceramic particles (WC particles) enter the molten pool at a lower speed, avoiding rushing into the bottom of the molten pool due to excessive speed, and at the same time alleviating the problem of sinking due to excessive density, resulting in the accumulation of hard ceramic particles (WC particles) in the coating.

[0045] Example 3: This patent also discloses a cladding gun head, which is used in the laser cladding method of the above-mentioned extruder barrel, including a gun head body 1, two nozzles 2 arranged opposite to each other on both sides of one end of the gun head body 1, a laser light source 8 located in the middle of the gun head body 1, a parabolic focusing copper mirror 6 arranged at the end of the gun head body 1 relative to the laser light source 8, and a powder delivery channel 3 respectively connected to the two nozzles 2, each of the nozzles 2 is respectively connected to two powder delivery channels 3, and the parabolic focusing copper mirror 6 can make the laser light emitted by the laser light source 8 be emitted from the middle of the two nozzles 2. In addition, a protective gas channel 4 and a cooling water channel 5 are also provided on the gun head body 1. In this example, argon gas with a purity of 99.99% is introduced into the protective gas channel 4 to protect the cladding molten pool, and 20°C cooling water is introduced into the cooling water channel 5 to reduce the working temperature of the gun head.

[0046] The working principle of the cladding gun head disclosed in this example is as follows: a beam of laser light source 8 forms two beams of light through a beam splitter prism 7, each beam of light is reflected by a parabolic focusing copper mirror 6 and reaches the inner wall of the workpiece (extruder barrel), and is matched with a powder feeding nozzle 2, one nozzle 2 delivers wear-resistant alloy powder, and the other nozzle 2 delivers non-wear-resistant alloy powder; for the nozzle 2 for delivering wear-resistant alloy powder, it includes two powder feeding channels 3, and different powder-carrying airflows are used to deliver nickel-chromium matrix powder and hard ceramic particles to the molten pool. During the working process, the actual workpiece only needs to be rotated 180 degrees, at which time half of the wear-resistant alloy coating and the other half of the non-wear-resistant ordinary alloy coating can be formed at one time.

[0047] The process design of the present invention is scientific and reasonable, convenient, efficient and easy to implement. In the actual laser cladding process, the actual workpiece only needs to be rotated 180 degrees to complete the one-time cladding of half-side wear-resistant alloy coating and half-side non-wear-resistant alloy coating on the inner wall of the extruder barrel, thereby maximizing the utilization of materials and effectively controlling costs. Compared with the traditional embedded alloy bushing, the alloy coating is metallurgically combined with the barrel to become one. At the same time, the wear resistance of the wear-resistant alloy coating disclosed in the present invention is much higher than that of the embedded alloy bushing, which effectively extends the service life and has a high application and promotion value.

[0048] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A laser cladding method for an extruder barrel, characterized in that: The inner wall of the extruder barrel is coated with a wear-resistant alloy coating on one side and a non-wear-resistant alloy coating on the other side, specifically comprising the following steps: S1. placing the cladding gun head at the center of the extruder barrel and moving the cladding gun head horizontally to the starting cladding position; S2. The upper and lower sides of the cladding gun head are respectively fed with powder to the molten pool; S3. The extruder barrel is rotated in a preset direction and angle so that half of the inner wall of the extruder barrel is clad with a wear-resistant alloy coating and half of the inner wall of the extruder barrel is clad with a non-wear-resistant alloy coating; The raw materials of the wear-resistant alloy coating are nickel-chromium matrix powder and raw materials for generating hard ceramic particles, the nickel-chromium matrix powder includes NiCr35 and Ti powder, the raw materials for generating hard ceramic particles include W powder and C powder, wherein the molar ratio of Ti powder, W powder and C powder is 1:1:2; The NiCr35 includes the following chemical components: C 0.5-0.6%, B 2.5-3.0%, Si 3.5-4.0%, Cr 13-14%, Fe4.5-5.5%, Ni BAL; The powder particle size of the NiCr35 is 50-105um, and the powder particle sizes of the Ti powder, W powder and C powder are 30-105um; The non-wear-resistant alloy coating is Fe35 powder, including the following chemical components: C 0.31%, B 1.11%, Si 1.22%, Cr17.6%, Ni 2.21%, Mn 0.20%, Fe BAL; In step S2, one side of the cladding gun head conveys nickel-chromium matrix powder, a raw material for generating hard ceramic particles, and the other side of the cladding gun head conveys Fe35 powder.

2. The laser cladding method for an extruder barrel according to claim 1, characterized in that: In step S2, the NiCr35 and Ti powders are ball-milled for 1 hour using a planetary ball mill, and nickel-chromium matrix powder is obtained after being evenly mixed; the nickel-chromium matrix powder and the raw materials for generating hard ceramic particles are then loaded into a V-type mixer and mixed for 30 minutes; and the powder is then delivered to the molten pool through the cladding gun head.

3. The laser cladding method for an extruder barrel according to claim 1, characterized in that: In step S2, one side of the cladding gun head includes two powder feeding channels, and different powder-carrying airflows are used to transport the nickel-chromium matrix powder and the raw materials for generating hard ceramic particles to the molten pool.

4. A cladding gun head, used in the laser cladding method of an extruder barrel according to claim 3, characterized in that: The invention comprises a gun head body (1), two nozzles (2) arranged opposite to each other at two sides of one end of the gun head body (1), a laser light source (8) located in the middle of the gun head body (1), a parabolic focusing copper mirror (6) arranged at the end of the gun head body (1) relative to the laser light source (8), and powder delivery channels (3) respectively connected to the two nozzles (2), each of the nozzles (2) being respectively connected to the two powder delivery channels (3), and the parabolic focusing copper mirror (6) enabling the laser light emitted by the laser light source (8) to be emitted from the middle of the two nozzles (2).

5. A cladding gun head according to claim 4, characterized in that: The gun head body (1) is also provided with a protective gas channel (4) and a cooling water channel (5).