A regeneration method for removing arsenic poisoning from spent SCR catalyst

Through dry cleaning, chemical cleaning and acid treatment, combined with the use of emulsifiers and oxidants, the problem of arsenic poisoning in SCR catalysts is solved, the mechanical strength recovery and performance improvement of the catalyst is achieved, and environmental pollution and toxicity groups are avoided. Introduce.

CN118577308BActive Publication Date: 2024-11-12ANHUI CONCH RESOURCES COMPREHENSIVE UTILIZATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410618316.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2024-11-12
Estimated Expiration
2044-05-17

AI Technical Summary

Technical Problem

Prior Art When treating arsenic poisoning in SCR catalysts, commonly used strong acid and alkali treatments will damage the mechanical strength of the catalyst. Calcium nitrate will introduce new toxic components and increase the cost of wastewater treatment, while persulfate is flammable and harmful to the human body. , difficult to use safely.

Method used

Using dry cleaning, pre-cleaning, chemical cleaning, acid cleaning and active loading, the arsenic element is removed and the catalyst is supplemented by acid treatment. The acidic site on the surface combines a composite solution of ammonium metavanadate, ammonium metatungstate and oxalic acid to activate the catalyst and finally undergoes heat treatment to restore the catalyst activity.

Benefits of technology

Effectively remove arsenic poisoning, restore the denitrification rate of the catalyst, improve the mechanical strength and performance of the catalyst, reduce environmental pollution, avoid the introduction of new toxic components, and reduce the cost of wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a regeneration method for removing arsenic poisoning from a waste SCR catalyst, which belongs to the technical field of SCR catalyst regeneration, and comprises the following steps: firstly performing dry cleaning and then water washing, and then performing chemical washing after water washing, and using a surfactant to remove the insoluble SiO 2 、A l 2 O 3 、CaSO 4 The catalyst surface is cleaned with a combination of hypochlorite and peracetic acid solution to produce oxidation, thereby removing arsenic that causes SCR catalyst poisoning, and then acid washing is performed to clean the pollutants that are easily soluble in water, while replenishing the acid sites on the catalyst surface to improve the performance of the catalyst. After the acid washing is completed, active impregnation loading is performed, drying and calcination treatment are performed, and finally the end is hardened to complete the regeneration. The regeneration method provided by the present invention is simple, and no new toxic components are introduced on the catalyst surface, and the obtained regenerated catalyst has good performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of SCR catalyst regeneration, and in particular relates to a regeneration method for removing arsenic poisoning from a waste SCR catalyst. Background Art

[0002] Selective catalytic reduction (SCR) denitrification technology has become the most widely used, most mature and most efficient flue gas denitrification technology due to its high denitrification efficiency, good selectivity, stable and reliable operation, etc. The catalyst is the core of SCR denitrification technology, and the performance of the catalyst directly affects the operating efficiency of the SCR denitrification system.

[0003] In actual operation, when high-arsenic coal is burned, the flue gas will contain a large amount of arsenic oxides, causing the SCR catalyst to be poisoned and deactivated, directly affecting the operating performance of the SCR denitrification system. In addition, the catalyst deactivated due to arsenic poisoning contains a large amount of arsenic oxides, which are hazardous wastes. How to economically and safely recycle and reuse the arsenic-poisoned catalyst is an urgent problem to be solved.

[0004] In order to solve the problem of arsenic poisoning of SCR catalyst, the Chinese patent with publication number CN102814201A adopts strong acid (H 2 SO4) and strong alkali (NaOH) are used alternately to clean the deactivated SCR denitration catalyst, thereby achieving the purpose of arsenic removal. The Chinese patent with publication number CN104857998B uses calcium nitrate and limestone to work together. The principle is that under alkaline conditions, the arsenic species on the catalyst surface will be free in the solution in the form of arsenous acid and arsenic acid. Then, by adding calcium ions to the solution, it reacts with arsenous acid and arsenic acid in the solution to produce calcium arsenite and calcium arsenate, thereby achieving the purpose of arsenic removal. The Chinese patent with publication number CN106732655A uses a persulfate solution with a neutral pH value as an oxidant to convert As 3+ Oxidized to easily soluble As 5+ Although the above patents have achieved certain technical effects, they still have the following shortcomings, such as: using strong acid and strong alkali to treat the deactivated SCR denitration catalyst will cause damage to the mechanical strength of the regenerated catalyst, reducing the service life of the SCR denitration catalyst; when calcium nitrate is used to clean the As poisoned catalyst, the cleaning liquid introduces a new toxic component-calcium ions to the catalyst surface, resulting in a large amount of waste liquid in the subsequent cleaning work, thereby increasing the cost of wastewater treatment; and although the use of persulfate to remove arsenic poisoning is more effective, persulfate itself is unstable, flammable, corrosive, irritating, can cause burns to the human body, and has high requirements for use and storage. Summary of the invention

[0005] The purpose of the present invention is to provide a regeneration method for removing arsenic poisoning from waste SCR catalysts. By reasonably controlling the raw material composition and ratio of the cleaning liquid, the denitration rate of the arsenic-poisoned SCR catalyst is restored, and the catalyst has good mechanical strength and less pollution to the environment.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A method for regenerating a waste SCR catalyst to remove arsenic poisoning comprises the following steps:

[0008] Step S1, dry deashing: mechanically deashing the arsenic-poisoned SCR catalyst module to obtain a deashed SCR catalyst;

[0009] Step S2, pre-cleaning and wet cleaning: The deashing SCR catalyst is pre-cleaned by flushing with process return water to remove dust on the catalyst surface and water-soluble salts, metal oxides, etc. in the catalyst, and then transferred to a cleaning tank, and cleaned by air bubbling with tap water to remove the ash blockage still remaining in the flow channel of the deashing SCR catalyst and the ash blockage in the gaps between catalyst units, thereby increasing the through-porosity of the deashing SCR catalyst and reducing the contamination of the subsequent cleaning liquid by the ash blockage. After the bubbling cleaning is completed, the catalyst is transferred to a draining tank for draining to obtain a clean SCR catalyst;

[0010] Step S3, chemical cleaning: an emulsifier, a penetrant, a peracetic acid solution and deionized water are uniformly mixed to obtain a first cleaning solution, and a clean SCR catalyst is added thereto, and the catalyst is cleaned by air bubbling ultrasonic cleaning at 40-100° C. for 0.5-4 hours, and then cleaned with tap water, and then transferred to a second cleaning solution, wherein the second cleaning solution is composed of an emulsifier, a penetrant, hypochlorite and deionized water, and the catalyst is cleaned by air bubbling ultrasonic cleaning at 40-100° C. for 0.5-4 hours, and then drained to obtain an arsenic-removed SCR catalyst;

[0011] The first cleaning solution and the second cleaning solution are composed of an emulsifier, a penetrant, hypochlorite, a peracetic acid solution and deionized water. On the one hand, the impurities adhering to the pores of the clean SCR catalyst are removed through emulsification, penetration, complexation and other mechanisms. On the other hand, the insoluble As 2 O 3 Oxidized to soluble As 2 O 5 , to achieve the removal of arsenic;

[0012] Step S4, acid cleaning: add sulfuric acid solution, deionized water and emulsifier S-185 into a cleaning tank, stir and mix evenly to obtain an acid cleaning solution, immerse the arsenic removal SCR catalyst in the acid cleaning solution, clean it with air bubbling ultrasonic at 40-100°C for 20-40min, and then transfer it to a draining tank for draining to obtain a deeply cleaned SCR catalyst;

[0013] Since the above chemical cleaning liquid contains hypochlorite, it is easy to introduce alkali metal and alkaline earth metal impurities on the surface of the arsenic removal SCR catalyst. Through acid cleaning, the water-soluble pollutants in the arsenic removal SCR catalyst are removed, and the acid sites on the catalyst surface are supplemented to improve the performance of the catalyst.

[0014] Step S5, active loading: ammonium metavanadate, ammonium metatungstate, oxalic acid and deionized water are mixed to obtain a composite solution, and the deep clean SCR catalyst is immersed in the composite solution at 40-100° C. for 0.5-2 h, and then transferred to a draining tank for draining to obtain an active supplemented SCR catalyst;

[0015] During the use of the catalyst, the active components will volatilize and lose due to mechanical wear, chemical action and other reasons. The catalyst needs to be supplemented with active substances. A reasonable active liquid formula is used to ensure that the active components are evenly and effectively loaded on the catalyst to improve the regeneration performance of the catalyst. The composite solution of the present invention mainly restores key active sites such as vanadium / tungsten on the surface of the catalyst, and oxalic acid can react to remove excess sodium hypochlorite added by chemical cleaning;

[0016] Step S6, heat treatment: drying and calcining the active supplementary SCR catalyst in a drying and calcining integrated kiln to remove moisture from the catalyst and activate the active components in the loading liquid, and then hardening the end to obtain a regenerated SCR catalyst.

[0017] Further, the mechanical dust removal steps are as follows:

[0018] The arsenic poisoned SCR catalyst module was treated with an ultrasonic soot blower to loosen the stubborn soot blockage, and then an air cannon was used to bombard it to remove the loose stubborn soot blockage, and finally compressed air was used to remove the floating soot on the surface.

[0019] Furthermore, the heat treatment drying temperature is 80-120°C, the drying time is 1-3h, the calcination temperature is 300-500°C, and the calcination time is 3-10h.

[0020] The main purpose of drying is to remove the surface moisture of the catalyst and ensure the mechanical strength of the catalyst. Calcination is carried out at high temperature, and its purpose is to react the loaded active components at high temperature to form an active chemical state and evenly disperse them on the catalyst surface, thereby ensuring that the deactivated catalyst recovers sufficient activity. The reaction is as follows:

[0021] 2NH 4 VO 3 ==V 2 O 5 +2NH 3 +H 2 O

[0022] H 28 N 6 O 41 W 12 ==12WO 3 +6NH 3 +5H 2 O.

[0023] Furthermore, the specific operation steps of end hardening are as follows:

[0024] The windward side of the dried and calcined active supplementary SCR catalyst is immersed in the hardening liquid for 5-10 seconds at room temperature, and then taken out and naturally air-dried.

[0025] Further, the hardening liquid is prepared by the following steps:

[0026] Add phosphoric acid, low-iron aluminum sulfate and vanadyl sulfate into deionized water and stir evenly. The mass ratio of phosphoric acid, low-iron aluminum sulfate, vanadyl sulfate and deionized water is 40-45:30-35:1-3:15-20. The Fe content in the low-iron aluminum sulfate is less than 20ppm.

[0027] Furthermore, the mass ratio of the emulsifier, the penetrant, the peracetic acid solution and the deionized water in the first cleaning solution is 0.1-0.5:0.1-0.5:1-2:100, and the mass fraction of the peracetic acid solution is 35%.

[0028] Furthermore, the mass ratio of the emulsifier, the penetrant, the hypochlorite and the deionized water in the second cleaning solution is 0.1-0.5:0.1-0.5:1-3:100.

[0029] Furthermore, the penetrant is one or more of JFC, sodium dodecylbenzene sulfonate, sodium dodecyl sulfonate, polyethylene glycol 200 and polyethylene glycol 300.

[0030] Furthermore, the emulsifier is one or more of lauryl alcohol polyoxyethylene ether, octylphenol polyoxyethylene ether and emulsifier S-185.

[0031] Furthermore, the hypochlorite is sodium hypochlorite and / or potassium hypochlorite.

[0032] Furthermore, in step S4, the mass fraction of the emulsifier S-185 in the acid cleaning solution is 0.005-1%, and the molar concentration of sulfuric acid is 0.2-0.8 mol / L.

[0033] Furthermore, in the composite solution of step S5, the mass ratio of ammonium metavanadate, ammonium metatungstate, oxalic acid and deionized water is 0.5-2:3-5:3-7:100.

[0034] Beneficial effects of the present invention:

[0035] 1. The present invention provides a regeneration method for removing arsenic poisoning from a waste SCR catalyst, which firstly performs dust cleaning, while increasing the through-hole rate of the catalyst module, reducing the pollution of the subsequent cleaning liquid caused by the dust blocking, washing away the particulate matter blocking the catalyst surface, the surface grease coating, and removing the soluble substances (K + 、Na + ), and then use surfactant to remove the insoluble SiO 2 、Al 2 O 3 、CaSO 4 For the removal of arsenic, a mixed solution of peracetic acid solution and hypochlorite is used to remove As 2 O 3 Oxidation produces soluble As 2 O 5 , and then pickling is performed to clean the water-soluble pollutants, while replenishing the acid sites on the catalyst surface to improve the performance of the catalyst. The regeneration method provided by the present invention is simple and will not introduce new toxic components on the catalyst surface. The obtained regenerated catalyst has good performance.

[0036] 2. The cleaning solution of the present invention is composed of an emulsifier, a penetrant, hypochlorite, a peracetic acid solution and deionized water, wherein both the hypochlorite and the peracetic acid solution have good oxidizing properties, and the two play a synergistic role in As 2 O 3 Oxidation produces soluble As 2 O 5 , remove the poisoning arsenic from the spent SCR catalyst. In addition, the peracetic acid solution also contains acetic acid molecules, which can chelate metal ions and help dissolve and remove arsenic ions.

[0037] 3. The mass ratio of the emulsifier, the penetrant, the peracetic acid solution and the deionized water in the first cleaning solution of the present invention is 0.1-0.5: 0.1-0.5: 1-2: 100, and the mass ratio of the emulsifier, the penetrant, the sodium hypochlorite and the deionized water in the second cleaning solution is 0.1-0.5: 0.1-0.5: 1-3: 100. By strictly controlling the dosage of the hypochlorite and the peracetic acid solution, it is helpful to remove the arsenic element that causes poisoning while retaining the original catalytic performance of the waste SCR catalyst. Specifically, the addition of too much hypochlorite and peracetic acid solution is likely to introduce excessive oxidation, resulting in the loss of the original active components of the waste SCR catalyst, such as vanadium, and the degradation of the catalytic performance. The addition of too little hypochlorite and peracetic acid solution is likely to cause insufficient oxidation, and a large amount of arsenic element that causes poisoning is not removed, which also causes the catalytic activity of the catalyst to be low. DETAILED DESCRIPTION

[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] Example 1

[0040] A method for regenerating a waste SCR catalyst to remove arsenic poisoning comprises the following steps:

[0041] Step S1, using a sonic soot blower to treat the arsenic poisoned SCR catalyst module to loosen the stubborn ash blockage, then using an air cannon to bombard it to remove the loose stubborn ash blockage, and finally using compressed air to remove the floating ash on the surface to obtain a deashed SCR catalyst;

[0042] Step S2, pre-cleaning the deashing SCR catalyst by flushing with process return water for 10 minutes, then transferring it to a cleaning tank, and cleaning it with tap water by air bubbling for 1 hour. After the bubbling cleaning is completed, transferring it to a draining tank for draining to obtain a clean SCR catalyst;

[0043] Step S3, the emulsifier, the penetrant, the peracetic acid solution (mass fraction of 35%) and the deionized water are mixed in a mass ratio of 0.1:0.1:1:100 to obtain a first cleaning liquid, the clean SCR catalyst is added, and the cleaning is carried out by air bubbling ultrasonic cleaning at 100°C for 0.5h, and then the cleaning is carried out with tap water, and then the cleaning is transferred to a second cleaning liquid, wherein the second cleaning liquid is composed of an emulsifier, a penetrant, a hypochlorite and deionized water in a mass ratio of 0.1:0.1:1:100, and the cleaning is carried out by air bubbling ultrasonic cleaning at 40°C for 4h, and then the cleaning is drained to obtain an arsenic-removing SCR catalyst;

[0044] Step S4, adding sulfuric acid solution, deionized water and emulsifier S-185 into a cleaning tank, stirring and mixing evenly to obtain an acid cleaning solution, wherein the mass fraction of emulsifier S-185 is 0.005%, and the molar concentration of sulfuric acid is 0.2 mol / L, immersing the arsenic removal SCR catalyst in the acid cleaning solution, and performing air bubbling ultrasonic cleaning at 40°C for 30 minutes, and then transferring the catalyst to a draining tank for draining to obtain a deeply cleaned SCR catalyst;

[0045] Step S5, ammonium metavanadate, ammonium metatungstate, oxalic acid and deionized water are mixed in a mass ratio of 0.5:3:3:100 to obtain a composite solution, and the deep clean SCR catalyst is immersed in the composite solution at 40° C. for 0.5 h, and then transferred to a draining tank for draining to obtain an active supplementary SCR catalyst;

[0046] Step S6, drying and calcining the active supplementary SCR catalyst in an integrated kiln, the drying temperature is 80°C, the drying time is 3h, the calcination temperature is 300°C, and the calcination time is 3h, then the windward side of the dried and calcined active supplementary SCR catalyst is immersed in hardening liquid at room temperature for 5s, taken out and naturally air-dried to obtain a regenerated SCR catalyst.

[0047] The hardening liquid is prepared by the following steps:

[0048] Add 45 kg of phosphoric acid, 35 kg of low-iron aluminum sulfate and 3 kg of vanadyl sulfate into 20 kg of deionized water and stir evenly. The Fe content in the low-iron aluminum sulfate is less than 20 ppm.

[0049] The penetrant is JFC, the emulsifier is lauryl alcohol polyoxyethylene ether, and the hypochlorite is sodium hypochlorite.

[0050] Example 2

[0051] A method for regenerating a waste SCR catalyst to remove arsenic poisoning comprises the following steps:

[0052] Step S1, using a sonic soot blower to treat the arsenic poisoned SCR catalyst module to loosen the stubborn ash blockage, then using an air cannon to bombard it to remove the loose stubborn ash blockage, and finally using compressed air to remove the floating ash on the surface to obtain a deashed SCR catalyst;

[0053] Step S2, pre-cleaning the deashing SCR catalyst by flushing with process return water for 15 minutes, then transferring it to a cleaning tank, and cleaning it by air bubbling with tap water for 1.5 hours. After the bubbling cleaning is completed, transferring it to a draining tank for draining to obtain a clean SCR catalyst;

[0054] Step S3, the emulsifier, the penetrant, the peracetic acid solution (mass fraction of 35%) and the deionized water are mixed in a mass ratio of 0.3:0.3:1.5:100 to obtain a first cleaning liquid, and the clean SCR catalyst is added, and the cleaning is carried out by air bubbling ultrasonic cleaning at 60°C for 2 hours, and then the cleaning is carried out with tap water, and then the cleaning is transferred to the second cleaning liquid, which is composed of an emulsifier, a penetrant, hypochlorite and deionized water in a mass ratio of 0.3:0.4:2:100, and the cleaning is carried out by air bubbling ultrasonic cleaning at 80°C for 3 hours, and then drained to obtain an arsenic-removing SCR catalyst;

[0055] Step S4, adding sulfuric acid solution, deionized water and emulsifier S-185 into the cleaning tank, stirring and mixing evenly to obtain an acid cleaning solution, wherein the mass fraction of the emulsifier S-185 is 0.008%, and the molar concentration of sulfuric acid is 0.6 mol / L, immersing the arsenic removal SCR catalyst in the acid cleaning solution, and performing air bubbling ultrasonic cleaning at 60°C for 30 minutes, and then transferring the catalyst to a draining tank for draining to obtain a deeply cleaned SCR catalyst;

[0056] Step S5, ammonium metavanadate, ammonium metatungstate, oxalic acid and deionized water are mixed in a mass ratio of 1:4:5:100 to obtain a composite solution, and the deep clean SCR catalyst is immersed in the composite solution at 60° C. for 1 hour, and then transferred to a draining tank for draining to obtain an active supplementary SCR catalyst;

[0057] Step S6, drying and calcining the active supplementary SCR catalyst in an integrated kiln, the drying temperature is 100°C, the drying time is 2 hours, the calcination temperature is 400°C, and the calcination time is 8 hours, then the windward side of the dried and calcined active supplementary SCR catalyst is immersed in hardening liquid at room temperature for 8 seconds, taken out and naturally air-dried to obtain the regenerated SCR catalyst.

[0058] The hardening liquid is prepared by the following steps:

[0059] Add 40kg of phosphoric acid, 30kg of low-iron aluminum sulfate and 1kg of vanadyl sulfate into 15kg of deionized water and stir evenly. The Fe content in the low-iron aluminum sulfate is less than 20ppm.

[0060] The penetrant is sodium dodecylbenzene sulfonate, the emulsifier is lauryl alcohol polyoxyethylene ether, and the hypochlorite is sodium hypochlorite.

[0061] Example 3

[0062] A method for regenerating a waste SCR catalyst to remove arsenic poisoning comprises the following steps:

[0063] Step S1, using a sonic soot blower to treat the arsenic poisoned SCR catalyst module to loosen the stubborn ash blockage, then using an air cannon to bombard it to remove the loose stubborn ash blockage, and finally using compressed air to remove the floating ash on the surface to obtain a deashed SCR catalyst;

[0064] Step S2, pre-cleaning the deashing SCR catalyst by flushing with process return water for 20 minutes, then transferring it to a cleaning tank, and cleaning it by air bubbling with tap water for 2 hours. After the bubbling cleaning is completed, transferring it to a draining tank for draining to obtain a clean SCR catalyst;

[0065] Step S3, the emulsifier, the penetrant, the peracetic acid solution (mass fraction of 35%) and the deionized water are mixed in a mass ratio of 0.5:0.5:2:100 to obtain a first cleaning liquid, and the clean SCR catalyst is added, and the cleaning is carried out by air bubbling ultrasonic cleaning at 40°C for 0.5h, and then washed with tap water, and then transferred to a second cleaning liquid, the second cleaning liquid is composed of an emulsifier, a penetrant, hypochlorite and deionized water in a mass ratio of 0.5:0.5:3:100, and the cleaning is carried out by air bubbling ultrasonic cleaning at 100°C for 0.5h, and then drained to obtain an arsenic-removing SCR catalyst;

[0066] Step S4, adding sulfuric acid solution, deionized water and emulsifier S-185 into a cleaning tank, stirring and mixing evenly to obtain an acid cleaning solution, wherein the mass fraction of the emulsifier S-185 is 0.005-1%, and the molar concentration of sulfuric acid is 0.8 mol / L, immersing the arsenic removal SCR catalyst in the acid cleaning solution, and performing air bubbling ultrasonic cleaning at 100°C for 40 minutes, and then transferring the catalyst to a draining tank for draining to obtain a deeply cleaned SCR catalyst;

[0067] Step S5, ammonium metavanadate, ammonium metatungstate, oxalic acid and deionized water are mixed in a mass ratio of 2:5:7:100 to obtain a composite solution, and the deep clean SCR catalyst is immersed in the composite solution at 100° C. for 2 hours, and then transferred to a draining tank for draining to obtain an active supplementary SCR catalyst;

[0068] Step S6, drying and calcining the active supplementary SCR catalyst in an integrated kiln, the drying temperature is 120°C, the drying time is 10 hours, the calcination temperature is 500°C, and the calcination time is 3 hours, then the windward side of the dried and calcined active supplementary SCR catalyst is immersed in a hardening liquid at room temperature for 10 seconds, taken out and naturally air-dried to obtain a regenerated SCR catalyst.

[0069] The hardening liquid is prepared by the following steps:

[0070] Add 42kg of phosphoric acid, 33kg of low-iron aluminum sulfate and 2kg of vanadyl sulfate into 18kg of deionized water and stir evenly. The Fe content in the low-iron aluminum sulfate is less than 20ppm.

[0071] The penetrant is sodium dodecyl sulfate, the emulsifier is octylphenol polyoxyethylene ether, and the hypochlorite is potassium hypochlorite.

[0072] Comparative Example 1

[0073] A method for regenerating a waste SCR catalyst to remove arsenic poisoning, compared with Example 1, only the operation of step S3 is adjusted as follows:

[0074] Step S3, the emulsifier, the penetrant, the peracetic acid solution (mass fraction of 35%) and the deionized water are mixed uniformly in a mass ratio of 0.1:0.1:1:100 to obtain a first cleaning solution, the clean SCR catalyst is added, and the cleaning is performed by air bubbling ultrasonic cleaning at 100° C. for 0.5 h, and then drained to obtain an arsenic-removing SCR catalyst;

[0075] The remaining raw materials and preparation process are the same as in Example 1.

[0076] Comparative Example 2

[0077] A method for regenerating a waste SCR catalyst to remove arsenic poisoning, compared with Example 1, only the operation of step S3 is adjusted as follows:

[0078] Step S3, adding the clean SCR catalyst into a second cleaning solution, wherein the second cleaning solution is composed of an emulsifier, a penetrant, hypochlorite and deionized water in a mass ratio of 0.1:0.1:1:100, and performing air bubbling ultrasonic cleaning at 40° C. for 4 h, and then draining to obtain an arsenic-removed SCR catalyst;

[0079] The remaining raw materials and preparation process are the same as in Example 1.

[0080] Comparative Example 3

[0081] A regeneration method for removing arsenic poisoning from a waste SCR catalyst. Compared with Example 1, the step S3 of Example 1, "mixing an emulsifier, a penetrant, a peracetic acid solution (mass fraction of 35%) and deionized water in a mass ratio of 0.1:0.1:1:100 to obtain a first cleaning solution" is replaced with "mixing an emulsifier, a penetrant, a peracetic acid solution (mass fraction of 35%) and deionized water in a mass ratio of 0.1:0.1:0.9:100 to obtain a first cleaning solution", and the remaining raw materials and preparation process are the same as Example 1.

[0082] Comparative Example 4

[0083] A regeneration method for removing arsenic poisoning from a waste SCR catalyst. Compared with Example 3, the step S3 of Example 1, "mixing an emulsifier, a penetrant, a peracetic acid solution (mass fraction of 35%) and deionized water in a mass ratio of 0.5:0.5:2:100 to obtain a first cleaning solution" is replaced with "mixing an emulsifier, a penetrant, a peracetic acid solution (mass fraction of 35%) and deionized water in a mass ratio of 0.5:0.5:2.5:100 to obtain a first cleaning solution", and the remaining raw materials and preparation process are the same as Example 3.

[0084] Comparative Example 5

[0085] A regeneration method for removing arsenic poisoning from a waste SCR catalyst. Compared with Example 1, the "second cleaning liquid consists of an emulsifier, a penetrant, hypochlorite and deionized water in a mass ratio of 0.1:0.1:1:100" in step S3 of Example 1 is replaced by "the second cleaning liquid consists of an emulsifier, a penetrant, hypochlorite and deionized water in a mass ratio of 0.1:0.1:0.9:100", and the remaining raw materials and preparation process are the same as Example 1.

[0086] Comparative Example 6

[0087] A regeneration method for removing arsenic poisoning from a waste SCR catalyst. Compared with Example 3, the "second cleaning liquid consists of an emulsifier, a penetrant, hypochlorite and deionized water in a mass ratio of 0.5:0.5:3:100" in step S3 of Example 3 is replaced by "the second cleaning liquid consists of an emulsifier, a penetrant, hypochlorite and deionized water in a mass ratio of 0.5:0.5:3.5:100", and the remaining raw materials and preparation process are the same as Example 3.

[0088] The regenerated SCR catalysts obtained in Examples 1 to 3 and Comparative Examples 1 to 6 were tested, and the denitration rate (%), relative activity (K / KO), SO 2 / SO 3 Oxidation rate (%), the results are shown in Table 1:

[0089]

[0090] It can be seen from Table 1 that compared with Comparative Examples 1-6, the denitration efficiency, relative activity and SO 2 / SO 3 The oxidation rates are good, proving that both hypochlorite and peracetic acid solutions have good oxidizing properties, the two play a synergistic role, and both excessive and insufficient amounts will cause adverse effects on the catalyst.

[0091] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0092] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for regenerating a waste SCR catalyst to remove arsenic poisoning, characterized in that: The following steps are involved: Step S1, mechanically removing ash from the arsenic-poisoned SCR catalyst module to obtain a removed ash SCR catalyst; Step S2, washing the deashed SCR catalyst, draining it, and obtaining a clean SCR catalyst; Step S3, the emulsifier, the penetrant, the peracetic acid solution and the deionized water are uniformly mixed to obtain a first cleaning solution, the clean SCR catalyst is added, and the cleaning is carried out by air bubbling ultrasonic cleaning at 40-100° C. for 0.5-4 hours, and then the cleaning is transferred to a second cleaning solution after being washed with tap water. The second cleaning solution consists of an emulsifier, a penetrant, hypochlorite and deionized water, and the cleaning is carried out by air bubbling ultrasonic cleaning at 40-100° C. for 0.5-4 hours, and then drained to obtain an arsenic-removing SCR catalyst; Step S4, mixing sulfuric acid solution, deionized water and emulsifier S-185 evenly to obtain an acid cleaning solution, immersing the arsenic removal SCR catalyst in the acid cleaning solution, and cleaning it by air bubbling ultrasonic cleaning at 40-100° C. for 20-40 minutes, and draining to obtain a deeply cleaned SCR catalyst; Step S5, mixing ammonium metavanadate, ammonium metatungstate, oxalic acid and deionized water to obtain a composite solution, immersing the deep clean SCR catalyst in the composite solution at 40-100° C. for 0.5-2 h, draining, and obtaining an active supplementary SCR catalyst; Step S6, drying and calcining the active supplementary SCR catalyst, and then hardening the end thereof to obtain a regenerated SCR catalyst; The mass ratio of the emulsifier, the penetrant, the peracetic acid solution and the deionized water in the first cleaning solution is 0.1-0.5:0.1-0.5:1-2:100, the mass fraction of the peracetic acid solution is 35%, and the mass ratio of the emulsifier, the penetrant, the hypochlorite and the deionized water in the second cleaning solution is 0.1-0.5:0.1-0.5:1-3:100; The hypochlorite is sodium hypochlorite and / or potassium hypochlorite; In step S3, the penetrant is one of JFC, sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate; In step S3, the emulsifier is octylphenol polyoxyethylene ether.

2. The method for regenerating a waste SCR catalyst to remove arsenic poisoning according to claim 1, characterized in that: The drying temperature is 80-120°C, the drying time is 1-3h, the calcination temperature is 300-500°C, and the calcination time is 3-10h.

3. The method for regenerating a waste SCR catalyst to remove arsenic poisoning according to claim 1, characterized in that: The specific steps for end hardening are as follows: The windward side of the dried and calcined active supplementary SCR catalyst is immersed in the hardening liquid for 5-10 seconds at room temperature, and then taken out and naturally air-dried.

4. The method for regenerating a waste SCR catalyst to remove arsenic poisoning according to claim 3, characterized in that: The hardening liquid is prepared by the following steps: Add phosphoric acid, low-iron aluminum sulfate and vanadyl sulfate into deionized water and stir evenly. The mass ratio of phosphoric acid, low-iron aluminum sulfate, vanadyl sulfate and deionized water is 40-45:30-35:1-3:15-20. The Fe content in the low-iron aluminum sulfate is less than 20ppm.

5. The method for regenerating a waste SCR catalyst to remove arsenic poisoning according to claim 1, characterized in that: In step S5, the mass ratio of ammonium metavanadate, ammonium metatungstate, oxalic acid and deionized water in the composite solution is 0.5-2:3-5:3-7:100.