An antibacterial purification inorganic lightweight decorative panel and preparation method thereof
Through atomization and uniform distribution of antibacterial materials and infrared treatment, the problem of surface adhesion of inorganic lightweight boards is solved, the adhesion and effect of antibacterial materials are improved, and the antibacterial purification function and decorative performance of inorganic lightweight boards are achieved.
Patent Information
- Application Number
- CN202411060498.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The surface decorative layer of existing inorganic lightweight boards is smooth and dense, making it difficult to stably attach antibacterial purification materials, and the coating method is difficult to balance both decorative performance and functionality, resulting in the attenuation or disappearance of the antibacterial purification function.
Antibacterial materials are planted on the surface of the incompletely cured topcoat layer using atomization and uniform distribution, and a pore structure is formed through infrared irradiation and leveling treatment to improve the adhesion and antibacterial effect of the antibacterial materials.
It significantly improves the adhesion and antibacterial effect of antibacterial materials, avoids sagging defects, and takes into account the decorative performance and functionality of the board.
Smart Images

Figure CN118577464B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of antibacterial inorganic lightweight panels, in particular to an antibacterial purification inorganic lightweight decorative panel and a preparation method thereof. Background Art
[0002] Pre-coated decorative panels based on inorganic lightweight boards have been widely used in building interior wall decoration. The boards have excellent decorative properties and have many advantages such as light weight, convenient construction, and green environmental protection, but they do not have the ability to actively inhibit or kill indoor pollutants and viruses and bacteria. Loading antibacterial purification materials on their surface and giving them functionality is one of the important ways to comprehensively control indoor pollutants. The existing technology usually adopts direct spraying or composite with the help of intermediate media. However, due to the smooth and dense decorative layer on the surface of the pre-coated board, it is difficult to stably attach the antibacterial purification material to the surface of the pre-coated decorative layer; and with daily cleaning and wiping, the functional layer will gradually wear and peel off, causing the antibacterial purification function to decay until it disappears; and, due to the large droplet size of the traditional coating method, the surface is prone to form visible particles and sagging defects, and it is difficult to take into account the decorative performance of the board while achieving functionality. At present, the above problems have not been well solved, which limits the implementation of this technology and the application of products. Summary of the invention
[0003] The object of the present invention is to provide an antibacterial and purifying inorganic lightweight decorative panel and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] A method for preparing an antibacterial and purifying inorganic lightweight decorative panel comprises the following steps:
[0006] S1, selecting an inorganic lightweight plate for pretreatment, coating the surface with topcoat after the pretreatment, and performing UV curing to form a first topcoat layer;
[0007] S2, continue to apply topcoat on the surface of the first topcoat layer formed in step S1, perform incomplete UV curing, and form a second topcoat layer;
[0008] S3, using an atomization uniform distribution method to plant the antibacterial material in the form of small droplets on the surface of the second topcoat layer formed in step S2, to form an uncured second topcoat layer with an antibacterial material layer, wherein the particle size of the small droplets of the antibacterial material is less than 10 um;
[0009] S4. The second topcoat layer obtained in step S3 and not fully cured and having antibacterial material is subjected to leveling treatment. During the leveling treatment, infrared irradiation is performed, and the surface temperature of the second topcoat layer is 35-50° C. The leveling treatment time is 5-15 min. After the leveling treatment, UV curing is performed again to obtain an antibacterial purification inorganic lightweight decorative panel.
[0010] Furthermore, the inorganic lightweight board in step S1 is one of gypsum board, calcium silicate board and fiber cement board, and the energy of ultraviolet light in UV curing in step S1 is 95-300mJ / cm 2 , the curing time is 4-12s.
[0011] Furthermore, the energy of the ultraviolet light in the incomplete UV curing in step S2 is 30-90 mJ / cm 2 , the curing time is 3-6s.
[0012] Furthermore, the energy of the ultraviolet light in the UV curing in step S4 is 500-1200 mJ / cm 2 , the curing time is 6-16s.
[0013] Furthermore, the topcoats used in the first topcoat layer formed in step S1 and the second topcoat layer formed in step S2 are both composed of polyurethane acrylate, tripropylene glycol diacrylate, a photoinitiator and a solvent, and the mass ratio of the polyurethane acrylate, tripropylene glycol diacrylate, the photoinitiator and the solvent is 10:2:1:16.
[0014] Furthermore, the solvent is a mixture of ethyl acetate, ethyl acetate and butanol, and the mass ratio of ethyl acetate, ethyl acetate and butanol is 5:7:4.
[0015] Furthermore, the antibacterial material in step S4 is prepared by the following method:
[0016] S101, ultrasonically dispersing nitrogen-doped nano-titanium dioxide into a mixed solution of vinyltrimethoxysilane, ethanol and deionized water, and soaking for 3 hours, and then washing with ethanol and vacuum drying at 20° C. for later use;
[0017] S102, dispersing the nitrogen-doped nano-titanium dioxide treated in step S101 into a mixed solution of epoxy polyacrylate, 1,6-hexanediol diacrylate, nonylphenol polyoxyethylene ether, a photoinitiator, ethyl acetate and butanol, and stirring and mixing for 1 hour to obtain a solution A;
[0018] S103, dissolving ammonium bicarbonate in deionized water to obtain solution B, blending solution A obtained in step S102 with solution B, and stirring for 0.5 h to obtain an antibacterial material.
[0019] Furthermore, in step S101, the mass ratio of nitrogen-doped nano-titanium dioxide, vinyltrimethoxysilane, ethanol and deionized water is 10:1:20:100.
[0020] Furthermore, the mass ratio of nitrogen-doped nano-titanium dioxide, epoxy polyacrylate, 1,6-hexanediol diacrylate, nonylphenol polyoxyethylene ether, photoinitiator, ethyl acetate and butanol in the A solution is 2:20:5:1:1:30:10, the mass ratio of ammonium bicarbonate and deionized water in the B solution is 1:8, and the mass ratio of the B solution to the A solution is 1:6.
[0021] An antibacterial and purifying inorganic lightweight decorative panel is prepared by the preparation method of the antibacterial and purifying inorganic lightweight decorative panel.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. In the present invention, the antibacterial material is sprayed on the surface of the UV coating when the UV coating is not completely cured, and the nitrogen-doped nano-titanium dioxide falls on the surface of the uncured coating in the form of droplets to form an antibacterial material layer, stably planting the antibacterial material on the surface of the plate, improving the adhesion of the functional layer, greatly improving the firmness of the antibacterial material on the surface of the coating, and not easy to fall off. The antibacterial purification material is dispersed into extremely fine particles and distributed on the surface of the plate by using atomization uniform distribution technology, avoiding the defects of sagging or visible particles on the surface of the plate, and taking into account the decorative performance while realizing the antibacterial purification function;
[0024] 2. In the process of coating the antibacterial material in the present invention, a semi-curing method is used for connection. This uneven cross-linking state makes it easier to form a pore structure inside the polymer material during curing. At the same time, the present invention uses infrared irradiation to cause the decomposition of ammonium bicarbonate and the volatilization of the solvent during the leveling treatment, which accelerates the formation of pores and makes it easier for nitrogen-doped nano-titanium dioxide to be inside the polymer material with a pore structure, thereby achieving a better antibacterial effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a process flow chart of the present invention;
[0026] Figure 2 The figure is a process flow chart for preparing the antibacterial material in the present invention. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] See also Figure 1 to Figure 2 , the present invention provides:
[0029] Example 1
[0030] A method for preparing an antibacterial and purifying inorganic lightweight decorative panel comprises the following steps:
[0031] S1. Select fiber cement board for pretreatment, apply topcoat on its surface after pretreatment, and perform UV curing. The energy of ultraviolet light in UV curing is 150mJ / cm 2 , the curing time is 6s, forming the first topcoat layer;
[0032] S2, continue to apply topcoat on the surface of the first topcoat layer formed in step S1, and perform incomplete UV curing. The energy of ultraviolet light in UV curing is 55mJ / cm 2 , the curing time is 4s, forming the second topcoat layer;
[0033] S3, using an atomization uniform distribution method to plant the antibacterial material in the form of small droplets on the surface of the second topcoat layer formed in step S2, to form an uncured second topcoat layer with an antibacterial material layer, wherein the particle size of the small droplets of the antibacterial material is 8 um;
[0034] S4, the second topcoat layer with antibacterial material obtained in step S3 which is not completely cured is subjected to leveling treatment. During the leveling treatment, the second topcoat layer is irradiated with infrared rays, and the surface temperature is 40° C. The leveling treatment time is 8 min. After the leveling treatment, UV curing is performed again. The energy of the ultraviolet light in the UV curing is 900 mJ / cm 2 The curing time is 11s, and an antibacterial and purifying inorganic lightweight decorative panel is obtained.
[0035] Example 2
[0036] A method for preparing an antibacterial and purifying inorganic lightweight decorative panel comprises the following steps:
[0037] S1. Select fiber cement board for pretreatment, apply topcoat on its surface after pretreatment, and perform UV curing. The energy of ultraviolet light in UV curing is 95mJ / cm 2 , the curing time is 4s, forming the first topcoat layer;
[0038] S2, continue to apply topcoat on the surface of the first topcoat layer formed in step S1, and perform incomplete UV curing. The energy of ultraviolet light in UV curing is 30mJ / cm 2 , the curing time is 3s, forming the second topcoat layer;
[0039] S3, using an atomization uniform distribution method to plant the antibacterial material in the form of small droplets on the surface of the second topcoat layer formed in step S2, to form an uncured second topcoat layer with an antibacterial material layer, wherein the particle size of the small droplets of the antibacterial material is 10 um;
[0040] S4, the second topcoat layer with antibacterial material obtained in step S3 which is not completely cured is subjected to leveling treatment. During the leveling treatment, the second topcoat layer is irradiated with infrared rays, and the surface temperature is 35° C. The leveling treatment time is 5 min. After the leveling treatment, UV curing is performed again. The energy of the ultraviolet light in the UV curing is 500 mJ / cm 2 , the curing time is 6s, and an antibacterial and purifying inorganic lightweight decorative panel is obtained.
[0041] Example 3
[0042] A method for preparing an antibacterial and purifying inorganic lightweight decorative panel comprises the following steps:
[0043] S1. Calcium silicate board is selected for pretreatment. After pretreatment, topcoat is applied on its surface and UV curing is performed. The energy of ultraviolet light in UV curing is 300mJ / cm 2 , the curing time is 12s, forming the first topcoat layer;
[0044] S2, continue to apply topcoat on the surface of the first topcoat layer formed in step S1, and perform incomplete UV curing. The energy of ultraviolet light in UV curing is 90mJ / cm 2 , the curing time is 6s, forming the second topcoat layer;
[0045] S3, using an atomization uniform distribution method to plant the antibacterial material in the form of small droplets on the surface of the second topcoat layer formed in step S2, to form an uncured second topcoat layer with an antibacterial material layer, wherein the particle size of the small droplets of the antibacterial material is 5 um;
[0046] S4, the second topcoat layer with antibacterial material obtained in step S3 which is not completely cured is subjected to leveling treatment. During the leveling treatment, the second topcoat layer is irradiated with infrared rays, and the surface temperature is 50° C. The leveling treatment time is 15 min. After the leveling treatment, UV curing is performed again. The energy of the ultraviolet light in the UV curing is 1200 mJ / cm 2 The curing time is 16s, and an antibacterial and purifying inorganic lightweight decorative panel is obtained.
[0047] Example 4
[0048] A method for preparing an antibacterial and purifying inorganic lightweight decorative panel comprises the following steps:
[0049] S1. Select a gypsum board for pretreatment, apply topcoat on its surface after pretreatment, and perform UV curing. The energy of ultraviolet light in UV curing is 200mJ / cm 2 , the curing time is 7s, forming the first topcoat layer;
[0050] S2, continue to apply topcoat on the surface of the first topcoat layer formed in step S1, and perform incomplete UV curing. The energy of ultraviolet light in UV curing is 60mJ / cm 2 , the curing time is 4s, forming the second topcoat layer;
[0051] S3, using an atomization uniform distribution method to plant the antibacterial material in the form of small droplets on the surface of the second topcoat layer formed in step S2, to form an uncured second topcoat layer with an antibacterial material layer, wherein the particle size of the small droplets of the antibacterial material is 10 um;
[0052] S4, the second topcoat layer with antibacterial material obtained in step S3 which is not completely cured is subjected to leveling treatment. During the leveling treatment, the second topcoat layer is irradiated with infrared rays, and the surface temperature is 40° C. The leveling treatment time is 10 min. After the leveling treatment, UV curing is performed again. The energy of the ultraviolet light in the UV curing is 1000 mJ / cm 2 , the curing time is 10s, and an antibacterial and purifying inorganic lightweight decorative panel is obtained.
[0053] The topcoats used for the first topcoat layer formed in step S1 and the second topcoat layer formed in step S2 in the above embodiment are both composed of polyaminoacrylate, tripropylene glycol diacrylate, a photoinitiator and a solvent. The photoinitiator uses 184 photoinitiator, and the solvent is a mixture of ethyl acetate, ethyl acetate and butanol. The specific configuration method is as follows: 40g of polyaminoacrylate, 8g of tripropylene glycol diacrylate, 4g of photoinitiator, 20g of ethyl acetate, 28g of ethyl acetate and 16g of butanol are mixed together and stirred evenly to obtain the above-mentioned raw materials for forming the first topcoat and the second topcoat.
[0054] The antibacterial material in the above embodiment is prepared by the following method:
[0055] S101, ultrasonically dispersing 2 g of nitrogen-doped nano-titanium dioxide into a mixed solution of 0.2 g of vinyltrimethoxysilane, 4 g of ethanol and 20 g of deionized water, and soaking the mixture for 3 h. After soaking, the mixture was washed with ethanol and vacuum dried at 20° C. for later use;
[0056] S102, dispersing the nitrogen-doped nano-titanium dioxide treated in step S101 into a mixed solution of 20 g epoxy polyacrylate, 5 g 1,6-hexanediol diacrylate, 1 g nonylphenol polyoxyethylene ether, 1 g photoinitiator, 30 g ethyl acetate and 10 g butanol, stirring and mixing for 1 hour to obtain solution A, wherein the photoinitiator can be 1173 photoinitiator;
[0057] S103, dissolving 1.3 g of ammonium bicarbonate in 10.2 g of deionized water to obtain solution B, blending solution A obtained in step S102 with solution B, and stirring for 0.5 h to obtain an antibacterial material.
[0058] In the above embodiments, the pretreatment of the inorganic lightweight board (gypsum board, calcium silicate board, fiber cement board) includes polishing, cleaning, degreasing and other pretreatments.
[0059] The nitrogen-doped nano-titanium dioxide is prepared by the following method:
[0060] Mix 120 ml of butyl titanate and 150 ml of isopropanol, add 180 ml of deionized water, then add acetic acid to adjust the pH to 2, stir and mix under sealed constant temperature conditions for 6 days, then adjust the pH to 10 with triethanolamine, react at 130°C for 20 hours, filter and wash, calcine at 500°C for 4 hours, and grind to obtain nitrogen-doped nano titanium dioxide.
[0061] Set the comparison ratio
[0062] Comparative Example 1
[0063] Compared with Example 1, the step S2 of Comparative Example 1 is changed. In step S2, complete UV curing is performed, and in step S3, the antibacterial material is evenly distributed on the surface of the completely cured second topcoat layer by atomizing. The remaining steps are exactly the same as in Example 1.
[0064] Comparative Example 2
[0065] Compared with Example 1, in Comparative Example 2, step S4 is changed, and the leveling and infrared irradiation processes in step S4 are cancelled. The remaining steps are exactly the same as those in Example 1.
[0066] Comparative Example 3
[0067] Compared with Comparative Example 1, Comparative Example 3 changes step S4, cancels the leveling and infrared irradiation treatments in step S4, and the remaining steps are exactly the same as those in Comparative Example 1.
[0068] Comparative Example 4
[0069] In Comparative Example 4, compared with Example 1, the preparation of the antibacterial material was changed, the preparation of solution B was cancelled, the nitrogen-doped nano-titanium dioxide was completely dispersed in solution A, and the remaining steps were exactly the same as in Example 1.
[0070] The antibacterial purification inorganic lightweight decorative panels prepared in the above Examples 1-4 and Comparative Examples 1-4 were tested for their antibacterial performance against Escherichia coli and Staphylococcus aureus, respectively. The test method was to culture the inoculated bacterial solution of Escherichia coli and Staphylococcus aureus, and the total number of colonies in the initial bacterial solution was 1.0×10 4 cfu / cm 2 The antibacterial purification inorganic lightweight decorative panels prepared in Examples 1-4 and Comparative Examples 1-4 were selected as samples, and after 24 hours of incubation, they were eluted with an eluent (the eluent was a phosphate saline eluent). The viable bacteria count and antibacterial rate of the eluent were calculated according to the national standard GB4789.2. The test results are shown in Tables 1 and 2 below:
[0071] Table 1: Antibacterial test table of antibacterial purification inorganic lightweight decorative panels prepared in Examples 1-4 and Comparative Examples 1-4 against Escherichia coli
[0072]
[0073] Table 2: Antibacterial test table of antibacterial purification inorganic lightweight decorative panels prepared in Examples 1-4 and Comparative Examples 1-4 against Staphylococcus aureus
[0074]
[0075] It can be seen from the data in Tables 1 and 2 above that the present invention can effectively improve the antibacterial properties of the material after introducing infrared irradiation and leveling treatment. At the same time, in the process of preparing the antibacterial material in the present invention, by introducing the B solution to decompose in the infrared irradiation process to generate gas, the solvent volatilization caused by the infrared irradiation can further guide the formation of pores and enhance the antibacterial properties of the material.
[0076] The adhesion of the antibacterial material layer in the antibacterial purification inorganic lightweight decorative panels prepared in the above Examples 1-4 and Comparative Examples 1-4 was tested, and the test was based on ISO grade. The test results are shown in Table 3 below:
[0077] Table 3: Adhesion grade test table of antibacterial materials in antibacterial purification inorganic lightweight decorative panels prepared in Examples 1-4 and Comparative Examples 1-4
[0078]
[0079] It can be seen from the data in Table 3 above that the antibacterial material is connected by a semi-curing method in the present invention, which greatly improves the adhesion between the antibacterial material and the coating. At the same time, in the specific treatment process, the adhesion of the antibacterial material is increased by infrared irradiation and leveling treatment liquid.
[0080] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing an antibacterial and purifying inorganic lightweight decorative panel, characterized in that: Use the following steps: S1, selecting an inorganic lightweight plate for pretreatment, coating the surface with topcoat after the pretreatment, and performing UV curing to form a first topcoat layer; S2, continue to apply topcoat on the surface of the first topcoat layer formed in step S1, perform incomplete UV curing, and form a second topcoat layer; S3, using an atomization uniform distribution method to plant the antibacterial material in the form of small droplets on the surface of the second topcoat layer formed in step S2, to form an uncured second topcoat layer with an antibacterial material layer, wherein the particle size of the small droplets of the antibacterial material is less than 10 um; S4, performing a leveling treatment on the second topcoat layer with antibacterial material obtained in step S3, wherein the surface temperature of the second topcoat layer is 35-50° C. by infrared irradiation during the leveling treatment, and the leveling treatment time is 5-15 min. After the leveling treatment, UV curing is performed again to obtain an antibacterial purification inorganic lightweight decorative panel; The antibacterial material in step S3 is prepared by the following method: S101, ultrasonically dispersing nitrogen-doped nano-titanium dioxide into a mixed solution of vinyltrimethoxysilane, ethanol and deionized water and soaking for 3 hours, washing with ethanol and vacuum drying at 20° C. for later use, wherein the mass ratio of the nitrogen-doped nano-titanium dioxide, vinyltrimethoxysilane, ethanol and deionized water is 10:1:20:100; S102, dispersing the nitrogen-doped nano-titanium dioxide treated in step S101 into a mixed solution of epoxy polyacrylate, 1,6-hexanediol diacrylate, nonylphenol polyoxyethylene ether, a photoinitiator, ethyl acetate and butanol, and stirring and mixing for 1 hour to obtain a solution A; S103, dissolving ammonium bicarbonate in deionized water to obtain solution B, blending solution A obtained in step S102 with solution B, and stirring for 0.5 h to obtain an antibacterial material.
2. The method for preparing the antibacterial purification inorganic lightweight decorative panel according to claim 1, characterized in that: The inorganic lightweight board in step S1 is one of gypsum board, calcium silicate board and fiber cement board. The energy of ultraviolet light in UV curing in step S1 is 95-300 mJ / cm 2 , the curing time is 4-12s.
3. The method for preparing the antibacterial purification inorganic lightweight decorative panel according to claim 1, characterized in that: The energy of the ultraviolet light in the incomplete UV curing in step S2 is 30-90 mJ / cm 2 , the curing time is 3-6s.
4. The method for preparing the antibacterial purification inorganic lightweight decorative panel according to claim 1, characterized in that: The energy of the ultraviolet light in the UV curing in step S4 is 500-1200 mJ / cm 2 , the curing time is 6-16s.
5. The method for preparing the antibacterial purification inorganic lightweight decorative panel according to claim 1, characterized in that: The topcoats used in the first topcoat layer formed in step S1 and the second topcoat layer formed in step S2 are both composed of polyurethane acrylate, tripropylene glycol diacrylate, photoinitiator and solvent, and the mass ratio of polyurethane acrylate, tripropylene glycol diacrylate, photoinitiator and solvent is 10:2:1:
16.
6. The method for preparing the antibacterial purification inorganic lightweight decorative panel according to claim 1, characterized in that: The mass ratio of nitrogen-doped nano-titanium dioxide, epoxy polyacrylate, 1,6-hexanediol diacrylate, nonylphenol polyoxyethylene ether, photoinitiator, ethyl acetate and butanol in the A solution is 2:20:5:1:1:30:10, the mass ratio of ammonium bicarbonate to deionized water in the B solution is 1:8, and the mass ratio of the B solution to the A solution is 1:
6.
7. An antibacterial and purifying inorganic lightweight decorative panel, characterized in that: The antibacterial purifying inorganic lightweight decorative panel is prepared according to the preparation method of any one of claims 1 to 6.