Calcined petroleum coke and its preparation method and application

By mixing petroleum coke with asphalt, CaO, and K2O, and using surfactants and soybean oil as dust removal and desulfurizers, the problems of high ash, high sulfur, and dust pollution are solved, and low ash, low sulfur, and high-density calcination are achieved. The production of petroleum coke has improved its adhesion and dust removal effect and expanded its application scope.

CN118579760BActive Publication Date: 2024-10-15ANHUI SHIHUA ENG & TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411076065.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-15
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing high-density calcined petroleum coke has high ash, high sulfur, unevenness and dust pollution problems during the production process, which affects its application and environmental safety.

Method used

By mixing petroleum coke with asphalt and CaO and K2O, and using cationic and anionic surfactants to stir and react with a dust removal and desulfurization agent made from soybean oil, acid treatment and high-temperature calcination are performed to form a low-ash, low-sulfur, high-density of calcined petroleum coke to improve its adhesion and dust removal effect.

Benefits of technology

It achieves the low ash, low sulfur and high density characteristics of calcined petroleum coke, enhances its bonding and crushing strength, reduces costs, effectively reduces dust pollution, and improves the purity and application prospects of the product.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a calcined petroleum coke and a preparation method and application thereof, and belongs to the technical field of petroleum coke. After the petroleum coke and asphalt are crushed, they are mixed with CaO and K2O for ball milling, reacted with acid, sprayed with dust removal and desulfurization agent, heated and stirred for reaction, volatilized, calcined, and granulated to obtain calcined petroleum coke. The density of the calcined petroleum coke obtained by the invention is greatly improved, the asphalt improves the adhesion of the calcined petroleum coke, the gap is small, the shrinkage stress is small, the crushing strength is large, the stability is good, the quality is uniform, the cost is low, the product purity is high, it has the characteristics of low ash, low sulfur, and high density, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of petroleum coke, and in particular to a calcined petroleum coke and a preparation method and application thereof. Background Art

[0002] Petroleum coke is a product obtained by separating the light and heavy oils from crude oil by distillation and then thermally cracking the heavy oil. From the appearance, coke is irregular in shape and black blocks (or particles) of different sizes with a metallic luster. The particles of coke have a porous structure. The main element is carbon, which accounts for more than 80wt%, and the rest are hydrogen, oxygen, nitrogen, sulfur and metal elements. Petroleum coke has its own unique physical, chemical and mechanical properties. The non-volatile carbon, volatile matter and mineral impurities (sulfur, water, ash, etc.) that generate heat determine the chemical properties of coke.

[0003] High-density calcined petroleum coke is mainly used as anode material for electrolytic aluminum. Its main characteristics are low ash, low sulfur, high density, nitrogen, phosphorus, iron and other trace elements. It is required to control these trace elements within 10 -6 % to 10 -5 %, and its various quality indicators have reached or exceeded the best similar products abroad. Among all the control indicators, high-density calcined petroleum coke has particularly strict requirements on the moisture content of coke, which is often required to be controlled below 0.5% or 0.3%. However, qualified finished coke needs to be further crushed and screened to be divided into different particle sizes to meet the particle size requirements of customers. Since coke has almost no moisture, dust will fly during the product stacking, loading and transportation, causing serious pollution and harmful to human health. Summary of the invention

[0004] The purpose of the present invention is to propose a calcined petroleum coke and its preparation method and application, the density of which is greatly improved, the asphalt improves the adhesion of the calcined petroleum coke, the gap is small, the shrinkage stress is small, the crushing strength is large, the stability is good, the quality is uniform, the cost is low, the product purity is high, it has the characteristics of low ash, low sulfur and high density, and has broad application prospects.

[0005] The technical solution of the present invention is achieved in this way:

[0006] The invention provides a preparation method of calcined petroleum coke. The method comprises the following steps: crushing petroleum coke and asphalt, mixing with CaO and K2O, and ball milling, wherein the mass ratio of the petroleum coke, asphalt, CaO and K2O is 10-20:1-2:3-5:1.5-2.5; reacting the product with an acid, wherein the acid is hydrochloric acid or sulfuric acid; spraying a dust removal and desulfurization agent, wherein the dust removal and desulfurization agent is a cationic surfactant and an anionic surfactant, adding the cationic surfactant and the anionic surfactant to soybean oil, stirring and mixing the mixture evenly, heating and stirring to react, volatilizing, calcining, and granulating the mixture to obtain the calcined petroleum coke.

[0007] As a further improvement of the present invention, the following steps are included:

[0008] S1. Pretreatment: After the petroleum coke and asphalt are crushed, they are mixed with CaO and K2O and ball-milled, acid is added and stirred for reaction, filtered, washed, and dried to obtain a pretreated material;

[0009] S2 dust removal and desulfurization agent preparation: the cationic surfactant, anionic surfactant was added to soybean oil, stirred and mixed to obtain a dust removal and desulfurization agent;

[0010] S3. Dust removal and desulfurization: Evenly spray the dust removal and desulfurization agent into the pretreated material, heat and stir the reaction to obtain treated petroleum coke;

[0011] S4 Calcination: The treated petroleum coke is calcined to obtain calcined petroleum coke;

[0012] S5. Granulation: The calcined petroleum coke is granulated by crushing and screening to obtain calcined petroleum coke with a particle size less than 10 mm.

[0013] As a further improvement of the present invention, the ball milling time in step S1 is 1-3h, the stirring reaction time is 20-30min, the acid is hydrochloric acid or sulfuric acid, and the acid concentration is 0.5-1.5mol / L; the mass ratio of petroleum coke, asphalt, CaO and K2O is 10-20:1-2:3-5:1.5-2.5.

[0014] As a further improvement of the present invention, the cationic surfactant in step S2 is selected from at least one of 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline, hexadecyltrimethylammonium bromide, and dodecyldimethylbenzylammonium chloride; the anionic surfactant is selected from at least one of sodium dodecylbenzenesulfonate, sodium dodecylsulfonate, sodium dodecyl sulfate, sodium tetradecylbenzenesulfonate, sodium tetradecyl sulfate, sodium tetradecylsulfonate, sodium hexadecylbenzenesulfonate, and sodium octadecylbenzenesulfonate, and the mass ratio of the cationic surfactant, the anionic surfactant, and the soybean oil is 7-10:3-5:100.

[0015] As a further improvement of the present invention, the cationic surfactant is 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline; and the anionic surfactant is sodium dodecylbenzene sulfonate.

[0016] As a further improvement of the present invention, the spraying amount of the dust removal and desulfurization agent in step S3 is 0.05-0.1wt%, the temperature of the heating and stirring reaction is 120-140°C, and the time is 1-2h.

[0017] As a further improvement of the present invention, the calcination temperature in step S4 is 1200-1300° C. and the calcination time is 2-4 hours.

[0018] As a further improvement of the present invention, the present invention specifically comprises the following steps:

[0019] S1. Pretreatment: 10-20 parts by weight of petroleum coke, 1-2 parts by weight of asphalt after crushing, mixed with 3-5 parts by weight of CaO and 1.5-2.5 parts by weight of K2O, ball milled for 1-3h, added with hydrochloric acid or sulfuric acid at a concentration of 0.5-1.5mol / L, stirred for 20-30min, filtered, washed and dried to obtain a pretreated material;

[0020] S2 dust removal and desulfurization agent preparation: 7-10 parts by weight of 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline, 3-5 parts by weight of sodium dodecylbenzene sulfonate were added to 100 parts by weight of soybean oil, stirred and mixed to obtain a dust removal and desulfurization agent;

[0021] S3. Dust removal and desulfurization: evenly spray the dust removal and desulfurization agent into the pretreated material at a spraying amount of 0.05-0.1wt%, heat to 120-140°C, stir and react for 1-2h to obtain treated petroleum coke;

[0022] S4. Calcination: The treated petroleum coke is heated to 1200-1300°C and calcined for 2-4h to obtain calcined petroleum coke;

[0023] S5. Granulation: The calcined petroleum coke is granulated by crushing and screening to obtain calcined petroleum coke with a particle size less than 10 mm.

[0024] The present invention further protects a calcined petroleum coke obtained by the above preparation method.

[0025] The present invention further protects the use of the above-mentioned calcined petroleum coke in preparing anode materials for electrolytic aluminum.

[0026] The present invention has the following beneficial effects:

[0027] The price of petroleum coke is low, but its high sulfur content greatly limits its application. Among them, sulfur mainly exists in petroleum coke in the form of thiophene, and is distributed in the carbon skeleton and aromatic ring. The structure is stable and difficult to remove. Calcined petroleum coke is mainly used as anode material for electrolytic aluminum. Its main characteristics are low ash and low sulfur. Usually, when petroleum coke is mixed with asphalt, it is easy to generate a lot of dust when crushed, which affects product quality and working environment.

[0028] The present invention adopts alkali, including calcium oxide and potassium oxide, to mix and ball-mill with a mixture of petroleum coke and asphalt, so that the sulfide is fully exposed, Ca and K are synergistically intercalated in the petroleum coke, the structure of the petroleum coke is adjusted, the graphite microcrystalline structure inside the petroleum coke is loosened, and the contact area between the sulfide and the dust removal and desulfurization agent is increased, which is helpful for subsequent desulfurization treatment.

[0029] The dust removal and desulfurization agent of the present invention comprises a cationic surfactant, an anionic surfactant and soybean oil, which avoids the problem that the water content in the dust removal agent is difficult to control, resulting in the water content of the final coke exceeding the standard. At the same time, soybean oil is used as a solvent. On the one hand, it can volatilize and decompose during the high-temperature calcination process, and the cationic surfactant and the anionic surfactant can also decompose at high temperature, which will not affect the purity of the final product. At the same time, it has a good adsorption effect on dust. At the same time, the cationic surfactant and the anionic surfactant can attract each other with the negatively charged sites and the positively charged sites on the surface of the dust, respectively, thereby improving the wettability and the adsorption rate of the dust, and achieving a good dust removal effect.

[0030] In addition, in the dust removal and desulfurization agent, the cationic surfactant 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline can combine well with acidic sulfides such as sulfur dioxide to form stable compounds. At the same time, soybean oil has good solubility in sulfur-containing organic matter such as thiophene, and can greatly improve the sulfur removal effect in the pretreated material after pretreatment.

[0031] The density of the calcined petroleum coke prepared by the present invention is greatly improved, the asphalt improves the adhesion of the calcined petroleum coke, the gap is small, the shrinkage stress is small, the crushing strength is large, the stability is good, the quality is uniform, the cost is low, the product purity is high, it has the characteristics of low ash, low sulfur and high density, and has broad application prospects. DETAILED DESCRIPTION

[0032] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] Petroleum coke, with a sulfur content of 2.2-2.7 wt%, was purchased from Tianjin Mingxintai Petrochemical Co., Ltd. Example 1

[0034] This embodiment provides a method for preparing calcined petroleum coke, which specifically comprises the following steps:

[0035] S1. Pretreatment: 10g of petroleum coke and 1g of asphalt were crushed, mixed with 3g of CaO and 1.5g of K2O and ball-milled for 1h, 0.5mol / L of hydrochloric acid was added and stirred for 20min, filtered, washed and dried to obtain a pretreated material;

[0036] S2 dust removal desulfurization agent preparation: The 7g 2-undecyl -N- carboxymethyl -N hydroxyethyl imidazoline, 3g sodium dodecylbenzene sulfonate was added to 100g soybean oil, stirred and mixed to obtain a dust removal desulfurization agent;

[0037] S3. Dust removal and desulfurization: evenly spray the dust removal and desulfurization agent into the pretreated material at a spraying amount of 0.05wt%, heat to 120°C, stir and react for 1h to obtain treated petroleum coke;

[0038] S4. Calcination: The treated petroleum coke is heated to 1200°C and calcined for 2h to obtain calcined petroleum coke;

[0039] S5. Granulation: The calcined petroleum coke is granulated by crushing and screening to obtain calcined petroleum coke with a particle size less than 10 mm. Example 2

[0040] This embodiment provides a method for preparing calcined petroleum coke, which specifically comprises the following steps:

[0041] S1 pretreatment: 20g of petroleum coke, 2g of asphalt after crushing, and 5g of CaO and 2.5g of K2O mixed ball milling 3h, added to a concentration of 1.5mol / L of sulfuric acid stirring reaction 30min, filtered, washed, dried to obtain a pretreated material;

[0042] S2 dust removal and desulfurization agent preparation: 10g 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline, 5g sodium dodecylbenzene sulfonate was added to 100g soybean oil, stirred and mixed to obtain a dust removal and desulfurization agent;

[0043] S3. Dust removal and desulfurization: evenly spray the dust removal and desulfurization agent into the pretreated material at a spraying amount of 0.1wt%, heat to 140°C, stir and react for 2h to obtain treated petroleum coke;

[0044] S4 Calcination: The treated petroleum coke is heated to 1300°C and calcined for 4 hours to obtain calcined petroleum coke;

[0045] S5. Granulation: The calcined petroleum coke is granulated by crushing and screening to obtain calcined petroleum coke with a particle size less than 10 mm. Example 3

[0046] This embodiment provides a method for preparing calcined petroleum coke, which specifically comprises the following steps:

[0047] S1 pretreatment: 15g of petroleum coke, 1.5g of asphalt after crushing, and 4g of CaO and 2g of K2O mixed ball milling 2h, adding a concentration of 1mol / L of hydrochloric acid stirring reaction 25min, filtered, washed, dried to obtain a pretreated material;

[0048] S2 dust removal desulfurization agent preparation: 8.5g 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline, 4g sodium dodecylbenzene sulfonate was added to 100g soybean oil, stirred and mixed to obtain a dust removal desulfurization agent;

[0049] S3. Dust removal and desulfurization: evenly spray the dust removal and desulfurization agent into the pretreated material at a spraying amount of 0.07wt%, heat to 130°C, stir and react for 1.5h to obtain treated petroleum coke;

[0050] S4. Calcination: The treated petroleum coke is heated to 1250°C and calcined for 3h to obtain calcined petroleum coke;

[0051] S5. Granulation: The calcined petroleum coke is granulated by crushing and screening to obtain calcined petroleum coke with a particle size of less than 10 mm.

[0052] Comparative Example 1

[0053] Compared with Example 3, the difference is that no alkali is added and no acid treatment is performed in step S1.

[0054] The details are as follows:

[0055] S1. Mixing: 15g of petroleum coke and 1.5g of asphalt were crushed to obtain a mixture;

[0056] S2 dust removal desulfurization agent preparation: 8.5g 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline, 4g sodium dodecylbenzene sulfonate was added to 100g soybean oil, stirred and mixed to obtain a dust removal desulfurization agent;

[0057] S3. Dust removal and desulfurization: evenly spray the dust removal and desulfurization agent into the mixture at a spraying amount of 0.07wt%, heat to 130°C, stir and react for 1.5h to obtain treated petroleum coke;

[0058] S4. Calcination: The treated petroleum coke is heated to 1250°C and calcined for 3h to obtain calcined petroleum coke;

[0059] S5. Granulation: The calcined petroleum coke is granulated by crushing and screening to obtain calcined petroleum coke with a particle size less than 10 mm.

[0060] Comparative Example 2

[0061] Compared with Example 3, the difference is that no 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline is added to the dust removal and desulfurization agent in step S2.

[0062] The details are as follows:

[0063] S1 pretreatment: 15g of petroleum coke, 1.5g of asphalt after crushing, and 4g of CaO and 2g of K2O mixed ball milling 2h, adding a concentration of 1mol / L of hydrochloric acid stirring reaction 25min, filtered, washed, dried to obtain a pretreated material;

[0064] S2 dust removal desulfurization agent preparation: 12.5g of sodium dodecylbenzene sulfonate was added to 100g of soybean oil, stirred and mixed to obtain a dust removal desulfurization agent;

[0065] S3. Dust removal and desulfurization: evenly spray the dust removal and desulfurization agent into the pretreated material at a spraying amount of 0.07wt%, heat to 130°C, stir and react for 1.5h to obtain treated petroleum coke;

[0066] S4. Calcination: The treated petroleum coke is heated to 1250°C and calcined for 3h to obtain calcined petroleum coke;

[0067] S5. Granulation: The calcined petroleum coke is granulated by crushing and screening to obtain calcined petroleum coke with a particle size less than 10 mm.

[0068] Comparative Example 3

[0069] Compared with Example 3, the difference is that sodium dodecylbenzene sulfonate is not added to the dust removal and desulfurization agent in step S2.

[0070] The details are as follows:

[0071] S1 pretreatment: 15g of petroleum coke, 1.5g of asphalt after crushing, and 4g of CaO and 2g of K2O mixed ball milling 2h, adding a concentration of 1mol / L of hydrochloric acid stirring reaction 25min, filtered, washed, dried to obtain a pretreated material;

[0072] S2 dust removal and desulfurization agent preparation: 12.5g 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline was added to 100g soybean oil, stirred and mixed to obtain a dust removal and desulfurization agent;

[0073] S3. Dust removal and desulfurization: evenly spray the dust removal and desulfurization agent into the pretreated material at a spraying amount of 0.07wt%, heat to 130°C, stir and react for 1.5h to obtain treated petroleum coke;

[0074] S4. Calcination: The treated petroleum coke is heated to 1250°C and calcined for 3h to obtain calcined petroleum coke;

[0075] S5. Granulation: The calcined petroleum coke is granulated by crushing and screening to obtain calcined petroleum coke with a particle size less than 10 mm.

[0076] Comparative Example 4

[0077] Compared with Example 3, the difference is that in step S2, no 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline and sodium dodecylbenzene sulfonate are added to the dust removal and desulfurization agent.

[0078] The details are as follows:

[0079] S1 pretreatment: 15g of petroleum coke, 1.5g of asphalt after crushing, and 4g of CaO and 2g of K2O mixed ball milling 2h, adding a concentration of 1mol / L of hydrochloric acid stirring reaction 25min, filtered, washed, dried to obtain a pretreated material;

[0080] S2. Preparation of dust removal and desulfurization agent: soybean oil is a dust removal and desulfurization agent;

[0081] S3. Dust removal and desulfurization: evenly spray the dust removal and desulfurization agent into the pretreated material at a spraying amount of 0.07wt%, heat to 130°C, stir and react for 1.5h to obtain treated petroleum coke;

[0082] S4. Calcination: The treated petroleum coke is heated to 1250°C and calcined for 3h to obtain calcined petroleum coke;

[0083] S5. Granulation: The calcined petroleum coke is granulated by crushing and screening to obtain calcined petroleum coke with a particle size less than 10 mm.

[0084] Test Example 1 Desulfurization Rate

[0085] The residual sulfur mass fraction of the calcined petroleum cokes prepared in Examples 1-3 and Comparative Examples 1-4 was measured using a microcomputer coulometric sulfur analyzer (CLS-3000), and the final desulfurization rate (%) of the petroleum coke was calculated according to the following formula. The results are shown in Table 1.

[0086] Desulfurization rate (%) = (w0-w1) / w0×100%

[0087] Wherein: w0 and w1 represent the sulfur mass fraction of petroleum coke and the residual sulfur mass fraction of calcined petroleum coke, respectively, %.

[0088] Table 1 ;

[0089] It can be seen from the above table that the calcined petroleum cokes prepared in Examples 1-3 of the present invention have a good desulfurization rate.

[0090] Test Example 2

[0091] The calcined petroleum cokes obtained in Examples 1-3 of the present invention and Comparative Examples 1-4 were tested for dust emission, and the results are shown in Table 2.

[0092] Table 2 ;

[0093] It can be seen from the above table that the calcined petroleum cokes prepared in Examples 1-3 of the present invention have better dust removal effects.

[0094] Test Example 3

[0095] The calcined petroleum cokes obtained in Examples 1-3 of the present invention and Comparative Examples 1-4 were subjected to performance testing.

[0096] Apparent porosity: tested according to the method of GB / T 4511.1-2008.

[0097] True specific gravity: tested according to the method of GB / T 4511.4-84.

[0098] The results are shown in Table 3.

[0099] Table 3 ;

[0100] It can be seen from the above table that the calcined petroleum cokes prepared in Examples 1-3 of the present invention have a larger density and a higher porosity.

[0101] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing calcined petroleum coke, It is characterized in that The following steps are involved: S1. Pretreatment: After the petroleum coke and asphalt are crushed, they are mixed with CaO and K2O and ball-milled, acid is added and stirred for reaction, filtered, washed, and dried to obtain a pretreated material; S2 dust removal and desulfurization agent preparation: the cationic surfactant, anionic surfactant was added to soybean oil, stirred and mixed to obtain a dust removal and desulfurization agent; S3. Dust removal and desulfurization: Evenly spray the dust removal and desulfurization agent into the pretreated material, heat and stir the reaction to obtain treated petroleum coke; S4 Calcination: The treated petroleum coke is calcined to obtain calcined petroleum coke; S5. Whole grain: The calcined petroleum coke is whole grained, crushed and sieved to obtain calcined petroleum coke having a particle size of less than 10 mm; The acid is hydrochloric acid or sulfuric acid, and the acid concentration is 0.5-1.5 mol / L; the mass ratio of petroleum coke, asphalt, CaO and K2O is 10-20:1-2:3-5:1.5-2.5; In step S2, the cationic surfactant is selected from at least one of 2-undecyl-N-carboxymethyl-N-hydroxyethylimidazoline, hexadecyltrimethylammonium bromide, and dodecyldimethylbenzylammonium chloride; the anionic surfactant is selected from at least one of sodium dodecylbenzenesulfonate, sodium dodecylsulfonate, sodium dodecyl sulfate, sodium tetradecylbenzenesulfonate, sodium tetradecyl sulfate, sodium tetradecylsulfonate, sodium hexadecylbenzenesulfonate, and sodium octadecylbenzenesulfonate, and the mass ratio of the cationic surfactant, the anionic surfactant, and the soybean oil is 7-10:3-5:

100.

2. The preparation method according to claim 1, characterized in that: The ball milling time in step S1 is 1-3 hours, and the stirring reaction time is 20-30 minutes.

3. The preparation method according to claim 1, characterized in that: The cationic surfactant is 2-undecyl-N-carboxymethyl-N-hydroxyethyl imidazoline; and the anionic surfactant is sodium dodecylbenzene sulfonate.

4. The preparation method according to claim 1, characterized in that: The spraying amount of the dust removal and desulfurization agent in step S3 is 0.05-0.1wt%, the temperature of the heating and stirring reaction is 120-140°C, and the time is 1-2h.

5. The preparation method according to claim 1, characterized in that: The calcination temperature in step S4 is 1200-1300° C. and the calcination time is 2-4 hours.

6. A calcined petroleum coke obtained by the preparation method according to any one of claims 1 to 5.

7. Use of the calcined petroleum coke as claimed in claim 6 in preparing anode materials for electrolytic aluminum.

Citation Information

Patent Citations

  • Petroleum coke based activated carbon for electrode material of supercapacitor, preparation method therefor and use thereof

    CN105236404A

  • Refinery coke modified low-grade coal-water slurry mixture and use thereof

    CN1275610A

  • Treatment of petroleum cokes to inhibit coke puffing

    EP0410050A2