Preparation method and application of chitosan diquaternary ammonium salt containing carbon-carbon double bonds

By introducing the quaternary ammonium salt structure of carbon-carbon double bonds into chitosan, the problems of insufficient water solubility and antibacterial performance of chitosan are solved, and the performance improvement in electromagnetic shielding composite materials and the swelling rate of water-absorbent resin are improved, which is suitable for in multiple fields.

CN118580397BActive Publication Date: 2024-10-01NAT REHABILITATION ASSISTIVE DEVICES RES CENT +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411077042.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-01
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The existing technology is difficult to improve the water solubility and antibacterial properties of chitosan, and its performance in electromagnetic shielding composite materials is insufficient.

Method used

Hydroxypropyltrimonium chloride chitosan was produced by reacting the etherifying agent 2,3-epoxypropyltrimonium chloride with chitosan, which was subsequently reacted with chloroacetyl chloride and 2-(methacrylic acid) Dimethylamino)ethyl ester reaction introduces carbon-carbon double bonds to form chitosan biquaternary ammonium salt containing carbon-carbon double bonds, thereby improving its water solubility and antibacterial properties.

Benefits of technology

The water solubility of chitosan is significantly improved, and the water absorption performance of the water-absorbent resin is improved. The synthesis steps are simple and the cost is low, and it is suitable for the fields of biology, medicine and chemical industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118580397B_ABST
    Figure CN118580397B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing and applying a chitosan bis-quaternary ammonium salt containing carbon-carbon double bonds. The structural formula of the chitosan bis-quaternary ammonium salt containing carbon-carbon double bonds is shown in formula (I) #imgabs0#. The synthesis steps of this invention are simple, the cost is low, and the required equipment and raw materials are readily available. It can effectively improve the swelling rate of water-absorbing resins and can be widely used in the fields of biology, medicine, materials, and chemical engineering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of medicine and chemical industry, and in particular to a preparation method and application of chitosan diquaternary ammonium salt containing carbon-carbon double bonds. Background Art

[0002] Chitosan is a natural polysaccharide. It is widely used in food, medicine, chemical industry and other fields because of its good biocompatibility, biotoxicity, biodegradability, antibacterial activity and antioxidant properties. The molecular structure of chitosan contains C2-NH2 and C6-OH with strong reactivity, which can be chemically modified. In order to improve the water solubility of chitosan and enhance the antibacterial properties of the molecule. Introducing quaternary ammonium salt structure into chitosan molecules has become one of the hot areas of chitosan derivative research. In order to better introduce quaternized chitosan into other reaction systems, it is necessary to synthesize a quaternized chitosan containing carbon-carbon double bonds. Summary of the invention

[0003] The purpose of the present invention is to provide a preparation method and application of chitosan diquaternary ammonium salt containing carbon-carbon double bonds, so as to solve the problems existing in the above-mentioned prior art and significantly improve the performance of electromagnetic shielding composite materials.

[0004] To achieve the above object, the present invention provides the following solutions:

[0005] The present invention comprises the following steps:

[0006] A. Adding etherifying agent 2,3-epoxypropyltrimethylammonium chloride to chitosan in a weight ratio of (2-4):1 to quaternize the chitosan to obtain hydroxypropyltrimethylammonium chloride chitosan;

[0007] B. dissolving the hydroxypropyltrimethylammonium chloride chitosan in N-methyl-2-pyrrolidone at a dissolution ratio of 0.025 g / ml to obtain a mixed solution, and reacting the mixed solution with chloroacetyl chloride at a volume ratio of 10:1 to obtain a chloroacetylated chitosan quaternary ammonium salt;

[0008] C dissolving the chloroacetylated chitosan quaternary ammonium salt in acetonitrile at a dissolution ratio of 0.002 g / mL to obtain an acetonitrile solution, reacting the acetonitrile solution with 2-(dimethylamino)ethyl methacrylate at a volume ratio of 25:1 to obtain a chitosan diquaternary ammonium salt containing a carbon-carbon double bond as a product represented by formula (I), wherein n is an average degree of polymerization in the range of 1000-2500;

[0009] Formula (I).

[0010] Furthermore, in step A, based on weight, the amount of the etherifying agent 2,3-epoxypropyltrimethylammonium chloride is 2-4 times the amount of chitosan; the amount of the chloroacetyl chloride is 3-5 times the amount of hydroxypropyltrimethylammonium chloride chitosan; and the amount of 2-(dimethylamino)ethyl methacrylate is 10-20 times the amount of chloroacetylated chitosan quaternary ammonium salt.

[0011] Furthermore, in step B, the hydroxypropyl trimethyl ammonium chloride chitosan is prepared by dispersing chitosan in a mixed solution of excess isopropanol and purified water, and then adding etherifying agent 2,3-epoxypropyl trimethyl ammonium chloride in an amount of 2-4 times the amount of chitosan, stirring and refluxing at 65-70°C for 5-7h, and the obtained solid is precipitated with anhydrous ethanol, filtered and dried to obtain hydroxypropyl trimethyl ammonium chloride chitosan; wherein the volume ratio of isopropanol to purified water is 1:(3-5).

[0012] Furthermore, the preparation method of the chloroacetylated chitosan quaternary ammonium salt comprises dispersing hydroxypropyl trimethyl ammonium chloride chitosan in an excess of 2-methyl-2-pyrrolidone, then slowly adding chloroacetyl chloride in an amount 3-5 times the amount of hydroxypropyl trimethyl ammonium chloride chitosan in a constant pressure closed system, stirring and reflux reacting at room temperature for 1-2 days, and then precipitating with an excess of isopropyl ether, filtering, and drying to obtain the chloroacetylated chitosan quaternary ammonium salt.

[0013] Furthermore, in step C, the chitosan diquaternary ammonium salt containing a carbon-carbon double bond is a chloroacetylated chitosan quaternary ammonium salt dispersed in an excess of acetonitrile, and then 10-20 times the amount of chloroacetylated chitosan quaternary ammonium salt is added with 2-(dimethylamino)ethyl methacrylate, and the mixture is stirred and refluxed at 55-60° C. for 12-24 hours, and then precipitated with an excess of isopropyl ether, filtered, and dried to obtain the chitosan diquaternary ammonium salt containing a carbon-carbon double bond.

[0014] The chitosan diquaternary ammonium salt containing carbon-carbon double bonds is used to increase the swelling rate of the water-absorbing resin.

[0015] The present invention discloses the following technical effects:

[0016] After the diquaternary ammonium salt group is introduced into the compound prepared by the invention, the water solubility is greatly improved compared with chitosan.

[0017] The invention can improve the water absorption performance of the water-absorbing resin when introduced into the water-absorbing resin, has simple synthesis steps, low cost, and easy-to-obtain required equipment and raw materials. The product obtained by the invention can be widely used in the fields of biology, medicine, materials and chemical industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 is the infrared spectrum of chitosan;

[0019] Figure 2 An infrared spectrum of hydroxypropyltrimethylammonium chloride chitosan is provided for an embodiment of the present invention;

[0020] Figure 3 Provide an infrared spectrum of chloroacetylated chitosan quaternary ammonium salt for an embodiment of the present invention;

[0021] Figure 4 Provide an infrared spectrum of a chitosan diquaternary ammonium salt containing a carbon-carbon double bond for an embodiment of the present invention; DETAILED DESCRIPTION

[0022] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0023] Unless otherwise specified, the "parts" described in the present invention are all based on mass parts.

[0024] Firstly, the more active C2-NH2 in chitosan is used to undergo a ring-opening reaction with the epoxy group of the etherifying agent 2,3-epoxypropyltrimethylammonium chloride to obtain hydroxypropyltrimethylammonium chloride chitosan, and then the C6-OH is quaternized and modified in two steps. The hydroxypropyltrimethylammonium chloride chitosan is dissolved in N-methyl-2-pyrrolidone and reacted with chloroacetyl chloride to obtain chloroacetylated chitosan quaternary ammonium salt, and then the chloroacetylated chitosan quaternary ammonium salt is dissolved in acetonitrile and reacted with 2-(dimethylamino)ethyl methacrylate to prepare chitosan diquaternary ammonium salt containing carbon-carbon double bonds.

[0025] The synthetic route of chitosan diquaternary ammonium salt containing carbon-carbon double bonds is as follows:

[0026]

[0027] Example 1

[0028] In this embodiment, the target compound chitosan diquaternary ammonium salt containing a carbon-carbon double bond is synthesized according to the above synthesis route.

[0029] 1) Preparation of hydroxypropyltrimethylammonium chloride chitosan: 2 g chitosan (see Figure 1 ) was dissolved in a mixed solvent of 15 ml isopropanol and 45 ml purified water, and then 6 g of etherifying agent 2,3-epoxypropyltrimethylammonium chloride was added. Stirring and refluxing reaction was carried out at 70°C for 6 hours. After the reaction was completed, precipitated with anhydrous ethanol, filtered and dried to obtain hydroxypropyltrimethylammonium chloride chitosan (see Figure 2 ).

[0030] like Figure 1 The infrared spectrum of chitosan is shown in Figure 1595cm -1 is the absorption peak of chitosan C2-NH2; Figure 2 As shown, the infrared spectrum of hydroxypropyltrimethylammonium chloride chitosan provided by the embodiment of the present invention is Figure 1 In comparison, 1595cm -1 The absorption peak of amino group disappeared and was replaced by 1480cm -1 represents the CH bending vibration and CN stretching vibration in the quaternary ammonium salt molecule and 3025cm -1 The four organic groups in the quaternary ammonium salt molecule will induce CH stretching vibration. The above analysis data proves that the synthesis of hydroxypropyltrimethylammonium chloride chitosan is successful.

[0031] 2) Preparation of chloroacetylated chitosan quaternary ammonium salt: 0.5 g hydroxypropyltrimethylammonium chloride chitosan (see Figure 2 ) was dissolved in 20 ml N-methylpyrrolidone, and then 2 ml chloroacetyl chloride was added to the constant pressure funnel and slowly dripped in. Under argon protection, the mixture was stirred and refluxed at room temperature for 24 hours. After the reaction, the mixture was precipitated with isopropyl ether, filtered and dried to obtain chloroacetylated chitosan quaternary ammonium salt (see Figure 3 ).

[0032] like Figure 3 As shown, the infrared spectrum of chloroacetylated chitosan quaternary ammonium salt is provided for the embodiment of the present invention, which is Figure 2 In comparison, at 755cm -1 A new absorption peak appears at , which is caused by the C-Cl stretching vibration introduced after the chloroacetylation reaction, indicating that the synthesis of chloroacetylated chitosan quaternary ammonium salt is successful.

[0033] 3) Preparation of chitosan diquaternary ammonium salt containing carbon-carbon double bonds: 0.1 g chloroacetylated chitosan quaternary ammonium salt (see Figure 3 ) was dissolved in 50 mL of acetonitrile, and then 2 ml of 2-(dimethylamino)ethyl methacrylate was added. The mixture was stirred and refluxed at 60°C for 12 h. After the reaction was completed, it was precipitated with isopropyl ether, filtered and dried to obtain chitosan diquaternary ammonium salt containing carbon-carbon double bonds (see Figure 4 ), in the diquaternary ammonium salt of chitosan containing carbon-carbon double bonds, n is the average degree of polymerization, and the value range is 1000-2500.

[0034] like Figure 4 As shown, the infrared spectrum of the chitosan diquaternary ammonium salt containing carbon-carbon double bonds is provided in the embodiment of the present invention, which is Figure 3 In comparison, the stronger 1650cm -1 The absorption peak at 755cm is C=C stretching vibration, and -1 The absorption peak at disappeared, indicating the successful introduction of C=C double bond and the successful quaternization reaction of Cl atom and tertiary amine group, indicating that the chitosan diquaternary ammonium salt containing carbon-carbon double bond was successfully synthesized.

[0035] Example 2

[0036] The difference from Example 1 is that:

[0037] 1) Preparation of hydroxypropyltrimethylammonium chloride chitosan: 2 g chitosan (see Figure 1 ) was dissolved in a mixed solvent of 15 ml isopropanol and 60 ml pure water, and then 4 g of etherifying agent 2,3-epoxypropyltrimethylammonium chloride was added. Stir and reflux at 65°C for 5 h. After the reaction, precipitate with anhydrous ethanol, filter and dry to obtain hydroxypropyltrimethylammonium chloride chitosan (see Figure 2 ).

[0038] 2) Preparation of chloroacetylated chitosan quaternary ammonium salt: 0.5 g hydroxypropyltrimethylammonium chloride chitosan (see Figure 2 ) was dissolved in 20 ml N-methylpyrrolidone, and then 1.5 ml chloroacetyl chloride was added to the constant pressure funnel and slowly dripped in. Under argon protection, the mixture was stirred and refluxed at room temperature for 24 hours. After the reaction, the mixture was precipitated with isopropyl ether, filtered and dried to obtain chloroacetylated chitosan quaternary ammonium salt (see Figure 3 ).

[0039] 3) Preparation of chitosan diquaternary ammonium salt containing carbon-carbon double bonds: 0.1 g chloroacetylated chitosan quaternary ammonium salt (see Figure 3 ) was dissolved in 50 mL of acetonitrile, and then 1 ml of 2-(dimethylamino)ethyl methacrylate was added. The mixture was stirred and refluxed at 55°C for 12 h. After the reaction was completed, it was precipitated with isopropyl ether, filtered and dried to obtain chitosan diquaternary ammonium salt containing carbon-carbon double bonds (see Figure 4 ).

[0040] Example 3

[0041] The difference from Example 1 is that:

[0042] 1) Preparation of hydroxypropyltrimethylammonium chloride chitosan: 2 g chitosan (see Figure 1 ) was dissolved in a mixed solvent of 15 ml isopropanol and 75 ml purified water, and then 8 g of etherifying agent 2,3-epoxypropyltrimethylammonium chloride was added. Stirring and reflux reaction was carried out at 70°C for 7 hours. After the reaction was completed, precipitated with anhydrous ethanol, filtered and dried to obtain hydroxypropyltrimethylammonium chloride chitosan (see Figure 2 ).

[0043] 2) Preparation of chloroacetylated chitosan quaternary ammonium salt: 0.5 g hydroxypropyltrimethylammonium chloride chitosan (see Figure 2) was dissolved in 20 ml N-methylpyrrolidone, and then 2.5 ml chloroacetyl chloride was added to the constant pressure funnel and slowly dripped in. Under argon protection, the mixture was stirred and refluxed at room temperature for 48 hours. After the reaction, the mixture was precipitated with isopropyl ether, filtered and dried to obtain chloroacetylated chitosan quaternary ammonium salt (see Figure 3 ).

[0044] 3) Preparation of chitosan diquaternary ammonium salt containing carbon-carbon double bonds: 0.1 g chloroacetylated chitosan quaternary ammonium salt (see Figure 3 ) was dissolved in 50 mL of acetonitrile, and then 2 ml of 2-(dimethylamino)ethyl methacrylate was added. The mixture was stirred and refluxed at 60°C for 24 h. After the reaction was completed, it was precipitated with isopropyl ether, filtered and dried to obtain chitosan diquaternary ammonium salt containing carbon-carbon double bonds (see Figure 4 ).

[0045] Determination of the swelling rate of N-isopropylacrylamide / 2-acrylamide-2-methylpropanesulfonic acid water-absorbing resin after adding chitosan diquaternary ammonium salt containing carbon-carbon double bonds:

[0046] Application Examples

[0047] 1.0% monomer mass fraction of chitosan diquaternary ammonium salt containing carbon-carbon double bonds is added to N-isopropylacrylamide / 2-acrylamide-2-methylpropanesulfonic acid water-absorbing resin, wherein the N-isopropylacrylamide / 2-acrylamide-2-methylpropanesulfonic acid water-absorbing resin comprises the following components in parts by weight: 80 parts of N-isopropylacrylamide, 20 parts of 2-acrylamide-2-methylpropanesulfonic acid, 1.5 parts of potassium persulfate, 0.5 parts of N,N-methylenebisacrylamide, 0.01 parts of N,N,N,N-tetramethylethylenediamine, 10 parts of calcium chloride, and 400 parts of water.

[0048] The preparation method of the water-absorbing resin specifically comprises the following steps: adding N-isopropyl acrylamide, 2-acrylamide-2-methylpropanesulfonic acid, 0.5% monomer mass fraction of chitosan diquaternary ammonium salt containing carbon-carbon double bonds, potassium persulfate, N,N-methylenebisacrylamide, N,N,N,N-tetramethylethylenediamine, calcium chloride and water into a reaction vessel equipped with a condensing device and a stirring device, adjusting the pH to 7 with a sodium hydroxide solution, heating to 35°C, mixing to obtain a gel-state resin, and then repeatedly washing with anhydrous ethanol and drying.

[0049] Blank example

[0050] This blank example is basically the same as the application example, except that the chitosan diquaternary ammonium salt containing a carbon-carbon double bond is not added.

[0051] Comparative Example 1

[0052] This comparative example is basically the same as the application example, except that 0.5% monomer mass fraction of chitosan diquaternary ammonium salt containing carbon-carbon double bonds is added.

[0053] Comparative Example 2

[0054] This comparative example is basically the same as the application example, except that 1.5% monomer mass fraction of chitosan diquaternary ammonium salt containing carbon-carbon double bonds is added.

[0055] Comparative Example 3

[0056] This comparative example is basically the same as the application example, except that 2.0% monomer mass fraction of chitosan diquaternary ammonium salt containing carbon-carbon double bonds is added.

[0057] Swelling rate test experiment:

[0058] The absorbent resin samples provided in the application example, blank example and comparative examples 1-3 were immersed in pure water for 12 hours, and their swelling ratios were measured after being taken out. The results are shown in Table 1.

[0059] Table 1 Comparison of swelling ratios of various implementation cases

[0060]

[0061] It can be seen from the above table that adding a certain amount of chitosan diquaternary ammonium salt containing carbon-carbon double bonds prepared in the present invention can effectively improve the swelling performance of the water-absorbing resin.

[0062] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing a chitosan diquaternary ammonium salt containing a carbon-carbon double bond, characterized in that: The following steps are involved: A. Adding etherifying agent 2,3-epoxypropyltrimethylammonium chloride to chitosan in a weight ratio of (2-4):1 to quaternize the chitosan to obtain hydroxypropyltrimethylammonium chloride chitosan; B. dissolving the hydroxypropyltrimethylammonium chloride chitosan in N-methyl-2-pyrrolidone at a dissolution ratio of 0.025 g / ml to obtain a mixed solution, and reacting the mixed solution with chloroacetyl chloride at a volume ratio of 10:1 to obtain a chloroacetylated chitosan quaternary ammonium salt; C dissolving the chloroacetylated chitosan quaternary ammonium salt in acetonitrile at a dissolution ratio of 0.002 g / mL to obtain an acetonitrile solution, reacting the acetonitrile solution with 2-(dimethylamino)ethyl methacrylate at a volume ratio of 25:1 to obtain a chitosan diquaternary ammonium salt containing a carbon-carbon double bond as a product represented by formula (I), wherein n is an average degree of polymerization in the range of 1000-2500; Formula (I).

2. The method for preparing a chitosan diquaternary ammonium salt containing a carbon-carbon double bond according to claim 1, wherein: In step B, the hydroxypropyl trimethyl ammonium chloride chitosan is prepared by dispersing chitosan in a mixed solution of excess isopropanol and purified water, and then adding etherifying agent 2,3-epoxypropyl trimethyl ammonium chloride in an amount of 2-4 times the amount of chitosan, stirring and refluxing at 65-70° C. for 5-7 hours, and the obtained solid is precipitated with anhydrous ethanol, filtered and dried to obtain hydroxypropyl trimethyl ammonium chloride chitosan; wherein the volume ratio of isopropanol to purified water is 1:(3-5).

3. The chitosan diquaternary ammonium salt prepared by the preparation method of the chitosan diquaternary ammonium salt containing carbon-carbon double bonds as claimed in claim 1 is used as an application to improve the swelling ratio of water-absorbing resin.