Atomic putty for special vehicle body material and preparation method thereof

By using putty cross-linked with terminal allyl borate and acrylate monomers on special body materials, the problems of low adhesion and environmental pollution of traditional putty are solved, achieving high adhesion, fast curing and safety. The coating performance of special body materials.

CN118580710BActive Publication Date: 2024-10-01GLEIHOW NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076685.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-01
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Traditional putties have low adhesion on special car body materials, and existing styrene-free unsaturated polyester resins will volatilize during use, resulting in environmental pollution and slow curing speed, affecting the adhesion of materials.

Method used

Terminal allyl borate and acrylate monomers are used as cross-linking monomers, combined with unsaturated polyester resin, hexagonal boron nitride and other ingredients to prepare special body materials with good air-drying properties and excellent bonding adhesion. Atomic ash.

Benefits of technology

The adhesion and air-drying properties of atomic ash are improved, and the flash point is higher than the maximum temperature of flammable liquids, ensuring product safety. Hexagonal boron nitride increases the thermal conductivity, reduces thermal expansion stress, and improves the lubrication effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention is a kind of putty for special vehicle body materials and a preparation method thereof, belonging to the technical field of coatings. The putty is composed of a main body putty and a curing agent, and the weight ratio of the main body putty to the curing agent is 100:1~3; the main body putty includes the following components by weight: 30~40 parts of unsaturated polyester resin; 2~5 parts of terminal allyl boric acid ethanolamine ester; 0.1~1 part of cobalt isooctanoate; 0.1~1 part of N,N-dimethylaniline; 0.1~1 part of organic bentonite; 0.5~3 parts of titanium dioxide; 1~5 parts of hexagonal boron nitride; 46~65 parts of talcum powder. The present invention also provides a preparation method of the above-mentioned putty. The putty for special vehicle body materials prepared by the present invention is free of styrene and has a high flash point. It has excellent adhesion to difficult-to-stick materials for special vehicle bodies, and solves the technical problems of putty for special vehicle body materials in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to putty for special vehicle body materials and a preparation method thereof. Background Art

[0002] Atomic putty is a kind of embedding material that has developed rapidly in recent years. It is mainly used to repair defects such as pits, pinholes, cracks, welds, etc. of various substrates to ensure the flatness and smoothness of the substrate surface before painting. Atomic putty is widely used in rail transit locomotives and the automobile industry, mainly used for the painting of complete vehicles and the repair of vehicle bodies. With the continuous development and breakthroughs of my country's rail transit industry and new energy vehicle industry, higher requirements have been put forward for vehicle body materials. Lightweight design materials, composite materials, functional materials, etc. have been widely used in rail transit, automobiles, new energy and special equipment. Traditional atomic putty has low adhesion on materials such as aluminum alloys, magnesium alloys, fiber composite materials, modified plastics, etc. Therefore, there is an urgent need for an atomic putty product suitable for special vehicle body materials.

[0003] In addition, some putties in the prior art are mainly based on styrene-type unsaturated polyester resins, which will volatilize a large amount of styrene when used, causing great harm to the human body and the environment. Some styrene-free unsaturated polyester putties use acrylate derivatives instead of styrene as cross-linking monomers, but they have low activity and slow reaction speed. Moreover, under normal temperature conditions, they have poor air drying properties and slow curing speed, which will cause problems such as long-term non-drying after coating, and also affect the adhesion of the putty to the material.

[0004] Therefore, it is necessary to develop a styrene-free special vehicle body material putty to solve the deficiencies in the prior art. Summary of the invention

[0005] The present invention aims at the above problems, makes up for the deficiencies of the prior art, and provides a putty for special vehicle body materials and a preparation method thereof. The present invention adopts terminal allyl borate and acrylic monomers instead of styrene as crosslinking monomers, and the prepared putty has good air drying properties and excellent bonding adhesion. In particular, it has an ideal bonding effect on difficult-to-bond materials such as aluminum alloys, magnesium alloys, fiber composite materials, and modified plastics.

[0006] The specific technical solutions are as follows:

[0007] A putty for special vehicle body materials, the putty is composed of main body putty and curing agent, the weight ratio of the main body putty to the curing agent is 100:1-3; the main body putty includes the following components in parts by weight:

[0008] 30-40 parts of unsaturated polyester resin;

[0009] 2-5 parts of terminal allyl boric acid ethanolamine ester;

[0010] 0.1~1 part of cobalt 2-ethylhexanoate;

[0011] 0.1~1 part of N,N-dimethylaniline;

[0012] 0.1~1 part of organic bentonite;

[0013] 0.5~3 parts of titanium dioxide;

[0014] 1-5 parts of hexagonal boron nitride;

[0015] 46~65 parts of talcum powder.

[0016] The hexagonal boron nitride used in the present invention is hexagonal boron nitride powder.

[0017] Another object of the present invention is to provide a method for preparing the above-mentioned atomic putty for special vehicle body materials, the preparation method being as follows: unsaturated polyester resin, terminal allyl boric acid ethanolamine ester, cobalt isooctanoate, and N,N-dimethylaniline are put into a reaction kettle, stirred evenly, and then organic bentonite, titanium dioxide, hexagonal boron nitride, and talcum powder are added in sequence, and stirring is continued for 40 to 60 minutes to obtain the main ash; the main ash is mixed evenly with the curing agent to obtain the above-mentioned atomic putty for special vehicle body materials. The reaction temperature of the above-mentioned preparation method is room temperature, and the stirring speed is 900 rpm.

[0018] Preferably, the unsaturated polyester resin is prepared according to the following steps: 30 parts of diethylene glycol, 17 parts of fumaric acid, 10 parts of nadic anhydride and 10 parts of tetrahydrophthalic anhydride are added into a reaction kettle according to weight parts, the temperature is raised to 200°C, and the reaction is carried out by heat preservation until the acid value is ≤40mgKOH / g, the vacuum pressure is controlled to be -0.09MPa, and vacuum dehydration is performed for 10min~20min; then the temperature is lowered to 120°C, 0.05 parts of a polymerization inhibitor is added; the temperature is further lowered to 90°C, 33 parts of hydroxyethyl methacrylate are added, the mixture is stirred evenly and the temperature is lowered to 50°C to obtain the unsaturated polyester resin.

[0019] Preferably, the terminal allyl boric acid ethanolamine ester is prepared according to the following steps: trimethylolpropane diallyl ether, ethanolamine and boric acid are placed in a reaction kettle in a weight ratio of 3.5:2:1; nitrogen is passed through and stirred, the temperature is raised to 170°C, and the temperature is kept for 5 to 6 hours for polycondensation reaction, and vacuum dehydration is performed for 0.5 to 1 hour and then the temperature is lowered to room temperature to obtain terminal allyl boric acid ethanolamine ester.

[0020] The beneficial effects of the present invention are as follows:

[0021] 1. The putty prepared by the present invention is styrene-free, has a flash point higher than the highest temperature of 93°C for flammable liquids in the "GB13690-2009 General Rules for Classification and Hazard Communication of Chemicals", and has no other physical and chemical hazards. The product is safer during storage, transportation and use;

[0022] 2. The terminal allyl boric acid ethanolamine ester in the present invention contains an allyl terminal group, which can improve the reactivity and reaction speed of the unsaturated polyester resin and hydroxyethyl methacrylate, provide an exogenous ligand for boron through the amino group on the side chain, and improve the compatibility of the filler and the polymer; at the same time, the reaction system contains two elements of boron and nitrogen, as well as active groups such as allyl, hydroxyl, and amino groups, and has a good adhesion effect on special car body materials and some difficult-to-adhere materials. Therefore, the putty prepared by the present invention has good adhesion, good air drying, and fast surface drying and curing speed;

[0023] 3. The present invention adds hexagonal boron nitride to the reaction system, which can increase the thermal conductivity of the putty, reduce the thermal expansion stress of the body material and the outer surface, improve the lubrication effect, and improve the polishing smoothness. DETAILED DESCRIPTION

[0024] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific implementation methods. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not used to limit the present invention.

[0025] Example 1: 30 parts of diethylene glycol, 17 parts of fumaric acid, 10 parts of nadic anhydride and 10 parts of tetrahydrophthalic anhydride were put into a reactor according to weight parts, heated to 200°C, and kept warm for reaction until the acid value reached 30 mgKOH / g, the vacuum pressure was controlled to be -0.09 MPa, and vacuum dehydration was performed for 10 min; then the temperature was lowered to 120°C, 0.05 parts of polymerization inhibitor was added; the temperature was further lowered to 90°C, 33 parts of hydroxyethyl methacrylate was added, stirred evenly and cooled to 50°C to obtain an unsaturated polyester resin.

[0026] 3.5 parts of trimethylolpropane diallyl ether, 2 parts of ethanolamine and 1 part of boric acid were placed in a reaction kettle; nitrogen was passed through and stirred, the temperature was raised to 170°C, and the temperature was kept for 5 hours for polycondensation reaction, and vacuum dehydration was performed for 0.5 hours and then cooled to room temperature to obtain terminal allyl boric acid ethanolamine ester.

[0027] 30 parts of unsaturated polyester resin, 2 parts of terminal allyl boric acid ethanolamine ester, 1 part of cobalt isooctanoate and 1 part of N,N-dimethylaniline prepared in the above steps are put into a reaction kettle, and after stirring evenly, 0.1 parts of organic bentonite, 0.5 parts of titanium dioxide, 1 part of hexagonal boron nitride and 65 parts of talc are added in sequence, and stirring is continued for 40 minutes to obtain the main ash.

[0028] Take 100 parts of the main ash prepared in the above steps and mix it with 1 part of benzoyl peroxide curing agent, the mass percentage of benzoyl peroxide is 50%, and mix them evenly to obtain atomic putty for special car body materials.

[0029] Example 2: 30 parts of diethylene glycol, 17 parts of fumaric acid, 10 parts of nadic anhydride and 10 parts of tetrahydrophthalic anhydride were put into a reactor according to weight parts, heated to 200°C, and kept warm for reaction until the acid value reached 35 mgKOH / g, the vacuum pressure was controlled to be -0.09 MPa, and vacuum dehydration was performed for 15 min; then the temperature was lowered to 120°C, 0.05 parts of a polymerization inhibitor was added; the temperature was further lowered to 90°C, 33 parts of hydroxyethyl methacrylate was added, stirred evenly and cooled to 50°C to obtain an unsaturated polyester resin.

[0030] According to weight parts, 7 parts of trimethylolpropane diallyl ether, 4 parts of ethanolamine and 2 parts of boric acid were put into a reaction kettle; nitrogen was passed through and stirred, the temperature was raised to 170°C, and the temperature was kept for 6 hours for polycondensation reaction, and vacuum dehydration was performed for 1 hour and then cooled to room temperature to obtain terminal allyl boric acid ethanolamine ester.

[0031] 35 parts of unsaturated polyester resin, 3 parts of terminal allyl boric acid ethanolamine ester, 0.5 parts of cobalt isooctanoate and 0.5 parts of N,N-dimethylaniline prepared in the above steps are put into a reaction kettle, and after stirring evenly, 0.2 parts of organic bentonite, 1 part of titanium dioxide, 2 parts of hexagonal boron nitride and 58 parts of talc are added in sequence, and stirring is continued for 60 minutes to obtain the main ash.

[0032] 100 parts of main ash and 2 parts of benzoyl peroxide curing agent are mixed, with the mass percentage of benzoyl peroxide being 55%, to obtain atomic ash for special vehicle body materials.

[0033] Example 3: 30 parts of diethylene glycol, 17 parts of fumaric acid, 10 parts of nadic anhydride and 10 parts of tetrahydrophthalic anhydride were put into a reactor according to weight parts, and the temperature was raised to 200°C for insulation reaction until the acid value reached 40 mgKOH / g. The vacuum pressure was controlled to be -0.09 MPa and vacuum dehydration was performed for 20 min; then the temperature was lowered to 120°C and 0.05 parts of polymerization inhibitor was added; the temperature was further lowered to 90°C, 33 parts of hydroxyethyl methacrylate was added, the mixture was stirred evenly and the temperature was lowered to 50°C to obtain an unsaturated polyester resin.

[0034] According to weight parts, 7 parts of trimethylolpropane diallyl ether, 4 parts of ethanolamine and 2 parts of boric acid were put into a reaction kettle; nitrogen was passed through and stirred, the temperature was raised to 170°C, and the temperature was kept for 6 hours for polycondensation reaction, and vacuum dehydration was performed for 1 hour and then cooled to room temperature to obtain terminal allyl boric acid ethanolamine ester.

[0035] 40 parts of unsaturated polyester resin, 5 parts of terminal allyl boric acid ethanolamine ester, 0.1 parts of cobalt isooctanoate and 0.1 parts of N,N-dimethylaniline are put into a reaction kettle and stirred evenly. Then, 1 part of organic bentonite, 3 parts of titanium dioxide, 5 parts of hexagonal boron nitride and 46 parts of talc are added in sequence. After stirring for 60 minutes, the main ash is obtained.

[0036] Take 100 parts of the main ash prepared above and mix it with 3 parts of benzoyl peroxide curing agent, the content of benzoyl peroxide is 52%, and mix them evenly to obtain atomic putty for special car body materials.

[0037] Comparative Example 1: The other steps are the same as those in Example 2, except that terminal allyl boric acid ethanolamine ester is not required to be prepared and terminal allyl boric acid ethanolamine ester is not added to the reaction system.

[0038] Comparative Example 2: The other steps are the same as those of Comparative Example 1, but 35 parts of styrene-based unsaturated polyester resin are added (35 parts of unsaturated polyester resin are added in Comparative Example 1).

[0039] The putties prepared in the above-mentioned Examples 1 to 3 and Comparative Examples 1 and 2 were subjected to performance tests, and the test results are shown in Table 1 below.

[0040] Table 1 Test data of each embodiment and each comparative example.

[0041]

[0042] It can be seen from Table 1 that the actual drying time and polishability of the putties prepared in Example 1, Example 2, and Example 3 are better than those in Comparative Example 1.

[0043] The adhesion of the putties prepared in Example 1, Example 2 and Example 3 to special materials is significantly better than that in Comparative Example 1 and Comparative Example 2.

[0044] The putties prepared in Example 1, Example 2 and Example 3 have high flash points, good air-drying properties, and are also superior in flexibility, impact resistance and adhesion, and can meet the use requirements of special vehicle body materials.

[0045] In summary, the present invention uses styrene-free unsaturated polyester resin as the main body, hydroxyethyl methacrylate as the active diluent monomer, and introduces terminal allyl boric acid ethanolamine ester to improve the reaction activity and adhesion. The prepared atomic putty has a significant effect on improving the surface coating performance of special body materials.

[0046] It can be understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.

Claims

1. A putty for special car body materials, characterized in that: The atomic putty is a styrene-free atomic putty, which is composed of a main body putty and a curing agent, wherein the weight ratio of the main body putty to the curing agent is 100:1-3; the main body putty includes the following components in parts by weight: 30-40 parts of unsaturated polyester resin; 2-5 parts of terminal allyl boric acid ethanolamine ester; 0.1~1 part of cobalt 2-ethylhexanoate; 0.1~1 part of N,N-dimethylaniline; 0.1~1 part of organic bentonite; 0.5~3 parts of titanium dioxide; 1-5 parts of hexagonal boron nitride; 46-65 parts of talc; The terminal allyl boric acid ethanolamine ester is prepared according to the following steps: trimethylolpropane diallyl ether, ethanolamine and boric acid are placed in a reaction kettle in a weight ratio of 3.5:2:1; nitrogen is passed through and stirred, the temperature is raised to 170°C, and the temperature is kept for 5 to 6 hours for polycondensation reaction, and vacuum dehydration is performed for 0.5 to 1 hour and then the temperature is lowered to room temperature to obtain the terminal allyl boric acid ethanolamine ester.

2. A method for preparing putty for special vehicle body materials according to claim 1, characterized in that: The preparation method is as follows: unsaturated polyester resin, terminal allyl boric acid ethanolamine ester, cobalt isooctanoate, and N,N-dimethylaniline are put into a reaction kettle, and after stirring evenly, organic bentonite, titanium dioxide, hexagonal boron nitride, and talcum powder are added in sequence, and stirring is continued for 40 minutes to 60 minutes to obtain main ash; the main ash is mixed evenly with a curing agent to obtain the atomic putty for special body materials according to claim 1.

3. The method for preparing putty for special vehicle body materials according to claim 2, characterized in that: The unsaturated polyester resin is prepared according to the following steps: 30 parts of diethylene glycol, 17 parts of fumaric acid, 10 parts of nadic anhydride and 10 parts of tetrahydrophthalic anhydride are added into a reaction kettle according to weight parts, the temperature is raised to 200° C., and the reaction is carried out by heat preservation until the acid value is 30 mgKOH / g-40 mgKOH / g, the vacuum pressure is controlled to be -0.09 MPa, and vacuum dehydration is carried out for 10 min-20 min; then the temperature is lowered to 120° C., 0.05 parts of a polymerization inhibitor is added; the temperature is further lowered to 90° C., 33 parts of hydroxyethyl methacrylate are added, the mixture is stirred evenly and the temperature is lowered to 50° C. to obtain the unsaturated polyester resin.