A fire-proof and stain-resistant nano-silicon anion coating and a preparation method thereof
By adding composite fillers to silicon negative ion coatings, using the combination of silicon microspheres and modified copolymer resins, the fire resistance and stain resistance of the coating are improved, and the negative ion release capacity is enhanced through the characteristics of titanium dioxide and tourmaline, which solves the existing solution The problem of insufficient performance of silicon negative ion coatings has achieved high-performance fire-resistant and stain-resistant effects.
Patent Information
- Application Number
- CN202411065839.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The existing silicon negative ion coatings have shortcomings in fire resistance and stain resistance, and their negative ion release capabilities are limited and cannot meet market demand.
By adding composite filler to the nano-silicon negative ion coating, silicone microspheres using precursor 2 as the core, the surface is connected to the modified copolymer resin through triazole groups. The modified copolymer resin is mainly modified polyborosilazane. The chain is polymerized with acrylic acid, ethyl acrylate and hexafluorobutyl methacrylate segments to form a comb-like structure on the surface of the coating, combined with the anti-fouling properties of the silicon coating, and improve the negative ion release effect through the characteristics of titanium dioxide and tourmaline.
It significantly improves the fire-resistant and stain-resistant performance and negative ion release capabilities of the paint, forming a good stain-resistant and fire-resistant ceramic layer to meet the market's demand for high-performance coatings.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of nano silicon anion coatings, and in particular to a fireproof and stain-resistant nano silicon anion coating and a preparation method thereof. Background Art
[0002] As people's pursuit of healthy life becomes more and more urgent, many companies have launched functional coatings that can release negative ions. Many of these products are endowed with negative ion releasing function by adding some negative ion additives. However, the negative ion release amount is low and the release time is limited, which can no longer meet the market demand. In the process of using, silicon negative ion coating will inevitably encounter various sudden fire situations, so it is required to have certain fireproof performance. At the same time, in order to meet the appearance requirements, it is also required to have good stain resistance. Summary of the invention
[0003] The purpose of the present invention is to provide a fireproof and stain-resistant nano silicon anion coating and a preparation method thereof, which solves the problem of insufficient fireproof and stain-resistant performance of existing silicon anion coatings and improves their anion release capacity.
[0004] The purpose of the present invention can be achieved by the following technical scheme: A method for preparing a fire-proof and stain-resistant nano-silicon anion coating, comprising the following steps: Step S1: weighing the following raw materials in parts by weight: 50-60 parts of silicone-acrylic emulsion, 8-10 parts of composite filler, 4-5 parts of nano-silicon dioxide, 0.5-1 parts of dispersant, 0.3-0.5 parts of defoamer, 1.5-2 parts of film-forming aid, 0.5 parts of thickener and 30-40 parts of deionized water;
[0005] Step S2: mixing the silicone-acrylic emulsion, the composite filler, nano-silicon dioxide, the dispersant, the defoaming agent, the film-forming aid, the thickener and the deionized water, stirring for 15-20 minutes at a stirring rate of 800-1000 rpm, to prepare a fire-resistant and stain-resistant nano-silicon anion coating;
[0006] The composite filler is prepared by the following steps:
[0007] Step A1: Tourmaline powder, dopamine and Tris-HCl buffer were mixed, ultrasonically dispersed for 30-40 minutes, and then reacted for 12 hours at a stirring rate of 60-80 rpm and room temperature to obtain precursor 1. Butyl titanate, glacial acetic acid and anhydrous ethanol were mixed, stirred at a stirring rate of 100-120 rpm and room temperature, and precursor 1 and hydrochloric acid solution were added, stirred for 30-40 minutes, and placed in an oven at a temperature of 80° C., baked for 12 hours, and then calcined at 450° C. for 3 hours to obtain precursor 2;
[0008] The pH of Tris-HCl buffer is 8.5, the dosage ratio of tourmaline powder, dopamine and Tris-HCl buffer is 2-3g: 0.006-0.007g: 300mL, the mass fraction of hydrochloric acid solution is 30%, and the dosage ratio of butyl titanate, glacial acetic acid, anhydrous ethanol, precursor 1 and hydrochloric acid solution is 8-10mL: 1-1.5mL: 35-40mL: 2-2.5g: 0.4mL;
[0009] During the reaction, under alkaline conditions, dopamine is wrapped on the surface of tourmaline powder to obtain precursor 1, and then titanium dioxide is deposited on the surface of precursor 1 by a sol-gel method using butyl titanate as a titanium source, and then calcined to obtain precursor 2;
[0010] Step A2: (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide were mixed, and the mixture was stirred at a rate of 120-140 rpm and a temperature of 90°C for 3-4 hours under nitrogen protection to obtain azidosilane. Precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane and deionized water were mixed, and ammonia water was added at a stirring rate of 150-200 rpm and room temperature to react for 2-3 hours. Then, azidosilane was added, and the reaction was continued for 1-1.5 hours. The mixture was spray-dried to obtain modified silicon microspheres.
[0011] The ratio of (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide is 3-3.2g: 3-3.2g: 60-70mL, the mass fraction of ammonia water is 25%, and the ratio of precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane, ammonia water and azidosilane is 6-7g: 0.04-0.05mol: 0.045-0.055mol: 20-24mL: 0.01-0.012mol;
[0012] During the reaction, under the action of sodium azide, the chlorine in (3-chloropropyl)triethoxysilane is azidated to form an azide group to obtain azide silane. Under alkaline conditions, the methoxy groups in dimethyldimethoxysilane and phenyltrimethoxysilane undergo hydrolysis and condensation to form an organic silicon microsphere structure with the precursor as the core. When azide silane is added, the azide silane also undergoes hydrolysis and condenses with the hydroxyl groups on the surface of the microspheres to obtain modified silicon microspheres containing azide groups on the surface.
[0013] Step A3: Modified silica microspheres, modified copolymer resin, copper sulfate and N,N-dimethylformamide are mixed, ultrasonically dispersed for 5-10 minutes, and under nitrogen protection, the stirring rate is 120-150 rpm, the temperature is 30° C., and pentamethyldiethylenetriamine is added with stirring, and the reaction is carried out for 24 hours to obtain a composite filler;
[0014] The dosage ratio of modified silica microspheres, modified copolymer resin, copper sulfate and pentamethyldiethylenetriamine is 12-14 g: 15-16 g: 3.2-3.4 g: 10-12 mL;
[0015] During the reaction, under the action of copper sulfate and pentamethyldiethylenetriamine as catalysts, the azide groups in the modified silicon microspheres and the alkyne groups in the modified copolymer resin undergo a click reaction to form a triazole structure, thereby connecting the modified copolymer resin to the modified silicon microspheres to obtain a composite filler.
[0016] The modified copolymer resin is prepared by the following steps:
[0017] Step B1: B-trichloroborazine, trimethylsilyl acetylene magnesium chloride solution and toluene are mixed, and the mixture is reacted for 4-6 hours under nitrogen protection, at a stirring rate of 100-120 rpm and a temperature of 30° C. to obtain alkynyl trichloroborazine; alkynyl trichloroborazine, methylvinyl dichlorosilane, dichlorosilane and dichloromethane are mixed, and the mixture is stirred at a stirring rate of 100-120 rpm and a temperature of -15° C., and ammonia is introduced, and the mixture is reacted for 3-4 hours to obtain modified polyborosilazane;
[0018] The molar concentration of trimethylsilyl acetylene magnesium chloride solution is 0.5 mol / L, the amount ratio of B-trichloroborazine and trimethylsilyl acetylene magnesium chloride solution is 0.06-0.065 mol: 110-120 mL, and the amount ratio of alkynyl trichloroborazine, methylvinyl dichlorosilane and dichlorosilane is 0.03-0.032 mol: 0.022-0.025 mol: 0.33-0.35 mol;
[0019] During the reaction, at a temperature of 30°C, the chlorine in B-trichloroborazine reacts with trimethylsilyl acetylene magnesium chloride solution to undergo a substitution reaction, thereby introducing a trimethylsilyl acetylene group to obtain alkynyl trichloroborazine, and the chlorine in alkynyl trichloroborazine, methylvinyl dichlorosilane and dichlorosilane undergoes a substitution reaction with ammonia to obtain a modified polyborosilazane containing a terminal double bond and a trimethylsilyl acetylene group.
[0020] Step B2: Mix modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, tetrahydrofuran and xylene, stir and add 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile at a stirring rate of 150-180 rpm and a temperature of 95° C., and react for 10-12 hours to obtain a copolymer resin, and mix the copolymer resin, potassium carbonate and methanol, and react for 1-2 hours at a stirring rate of 150-180 rpm and room temperature to obtain a modified copolymer resin;
[0021] The amount ratio of modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile is 10-12g: 15g: 50-55g: 20-25g: 2-3g: 6-8g, and the amount ratio of copolymer resin and potassium carbonate is 22-25g: 16-17g;
[0022] During the reaction, under the action of 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile, double bonds in the modified polyborosilazane, acrylic acid, ethyl acrylate and hexafluorobutyl methacrylate undergo free radical polymerization to obtain a copolymer resin, and trimethylsilyl acetylene in the copolymer resin undergoes deprotection under the action of potassium carbonate to form an alkynyl group to obtain a modified copolymer resin;
[0023] Beneficial effects of the invention: The invention discloses a fireproof and stain-resistant nano-silicon anion coating, which solves the problem of insufficient fireproof and stain-resistant performance of the existing silicon anion coating by adding a composite filler into the raw material of the nano-silicon anion coating, and also improves its anion release capacity; the composite filler is an organic silicon microsphere with a precursor 2 as the core, and a modified copolymer resin is connected to the surface through a triazole group, and the modified copolymer resin is based on a modified polyborosilazane as the main chain, and is polymerized with acrylic acid, ethyl acrylate and hexafluorobutyl methacrylate chain segments, because a large amount of fluorine exists in hexafluorobutyl methacrylate, these fluorines cause the copolymerized chain segments to migrate to the coating surface during the coating curing process, thereby forming a comb-like structure on the coating surface, which has a good anti-fouling effect, and is combined with the anti-fouling performance of the silicon coating itself, It has good anti-fouling performance. Since precursor 2 is based on tourmaline as the core with titanium dioxide attached to the surface, and titanium dioxide is a material that is easily exposed to sunlight to produce electrons, this effect is combined with the characteristics of tourmaline itself, thereby exerting a better negative ion release effect. In addition, since its external packaging structure contains a large number of triazole structures, these structures can also synergize with it to promote the release of negative ions. In the event of a fire, under the action of high temperature, the organic silicon microsphere structure formed by the composite filler will combine with the modified polyborosilazane chain segment to undergo a ceramic transformation. Due to the special B-trichloroborazine structure in the modified polyborosilazane, it will guide the organic silicon microsphere structure to combine with the modified polyborosilazane to form a continuous fireproof ceramic layer, thereby exerting a good coating fireproof effect. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1 A method for preparing a fireproof and stain-resistant nano-silicon anion coating comprises the following steps: Step S1: Weigh the following raw materials in parts by weight: 50 parts of commercial Yoshida silicone acrylic emulsion, 8 parts of composite filler, 4 parts of commercial TSP-L20 nano-silicon dioxide, 0.5 parts of commercial 7500W dispersant, 0.3 parts of commercial LKXP001 defoamer, 1.5 parts of commercial EPH film-forming aid, 0.5 parts of commercial TT-40 thickener and 30 parts of deionized water;
[0026] Step S2: mixing the silicone-acrylic emulsion, the composite filler, nano-silicon dioxide, the dispersant, the defoaming agent, the film-forming aid, the thickener and the deionized water, stirring for 15 minutes at a stirring rate of 800 rpm, to prepare a fire-resistant and stain-resistant nano-silicon anion coating;
[0027] The composite filler is prepared by the following steps:
[0028] Step A1: Mix commercially available 1250 mesh tourmaline powder, dopamine and Tris-HCl buffer, ultrasonically disperse for 30 minutes, and then react for 12 hours at a stirring rate of 60 rpm and room temperature to obtain precursor 1, mix butyl titanate, glacial acetic acid and anhydrous ethanol, stir at a stirring rate of 100 rpm and room temperature, add precursor 1 and hydrochloric acid solution, stir for 30 minutes, put into an oven at a temperature of 80°C, bake for 12 hours, and then calcine at 450°C for 3 hours to obtain precursor 2;
[0029] The pH of Tris-HCl buffer is 8.5, the dosage ratio of tourmaline powder, dopamine and Tris-HCl buffer is 2g:0.006g:300mL, the mass fraction of hydrochloric acid solution is 30%, and the dosage ratio of butyl titanate, glacial acetic acid, anhydrous ethanol, precursor 1 and hydrochloric acid solution is 8mL:1mL:35mL:2g:0.4mL;
[0030] Step A2: (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide were mixed, and reacted for 3 hours at a stirring rate of 120 rpm and a temperature of 90°C under nitrogen protection to obtain azidosilane. Precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane and deionized water were mixed, and stirred at a stirring rate of 150 rpm and room temperature, and ammonia water was added to react for 2 hours. Then, azidosilane was added, and the reaction was continued for 1 hour. The mixture was spray-dried to obtain modified silicon microspheres.
[0031] The ratio of (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide is 3g:3g:60mL, the mass fraction of ammonia water is 25%, and the ratio of precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane, ammonia water and azidosilane is 6g:0.04mol:0.045mol:20-24mL:0.01mol;
[0032] Step A3: Modified silica microspheres, modified copolymer resin, copper sulfate and N,N-dimethylformamide were mixed, ultrasonically dispersed for 5 minutes, and under nitrogen protection, a stirring rate of 120 rpm and a temperature of 30° C., pentamethyldiethylenetriamine was added and reacted for 24 hours to obtain a composite filler;
[0033] The amount ratio of modified silica microspheres, modified copolymer resin, copper sulfate and pentamethyldiethylenetriamine is 12g:15g:3.2g:10mL;
[0034] The modified copolymer resin is prepared by the following steps:
[0035] Step B1: B-trichloroborazine, trimethylsilyl acetylene magnesium chloride solution and toluene are mixed, and the mixture is reacted for 4 hours under nitrogen protection, at a stirring rate of 100 rpm and a temperature of 30°C to obtain alkynyl trichloroborazine; alkynyl trichloroborazine, methylvinyl dichlorosilane, dichlorosilane and dichloromethane are mixed, and the mixture is stirred at a stirring rate of 100 rpm and a temperature of -15°C, and ammonia is introduced, and the mixture is reacted for 3 hours to obtain modified polyborosilazane;
[0036] The molar concentration of trimethylsilyl acetylene magnesium chloride solution is 0.5 mol / L, the amount ratio of B-trichloroborazine and trimethylsilyl acetylene magnesium chloride solution is 0.06 mol:110 mL, and the amount ratio of alkynyl trichloroborazine, methylvinyl dichlorosilane and dichlorosilane is 0.03 mol:0.022 mol:0.33 mol;
[0037] Step B2: Modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, tetrahydrofuran and xylene are mixed, stirred at a stirring rate of 150 rpm and a temperature of 95° C., 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile are added, and the mixture is reacted for 10 hours to obtain a copolymer resin, and the copolymer resin, potassium carbonate and methanol are mixed, and the mixture is reacted for 1 hour at a stirring rate of 150 rpm and room temperature to obtain a modified copolymer resin;
[0038] The amount ratio of modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile is 10g:15g:50g:20g:2g:6g, and the amount ratio of copolymer resin and potassium carbonate is 22g:16g.
[0039] Example 2 A method for preparing a fireproof and stain-resistant nano-silicon anion coating comprises the following steps: Step S1: Weigh the following raw materials in parts by weight: 60 parts of commercial Yoshida silicone acrylic emulsion, 8 parts of composite filler, 5 parts of commercial TSP-L20 nano-silicon dioxide, 1 part of commercial 7500W dispersant, 0.5 parts of commercial LKXP001 defoamer, 1.5 parts of commercial EPH film-forming aid, 0.5 parts of commercial TT-40 thickener and 40 parts of deionized water;
[0040] Step S2: mixing the silicone-acrylic emulsion, the composite filler, nano-silicon dioxide, the dispersant, the defoaming agent, the film-forming aid, the thickener and the deionized water, stirring for 20 minutes at a stirring rate of 1000 rpm, to prepare a fire-resistant and stain-resistant nano-silicon anion coating;
[0041] The composite filler is prepared by the following steps:
[0042] Step A1: Mix commercially available 1250 mesh tourmaline powder, dopamine and Tris-HCl buffer, disperse by ultrasonication for 40 minutes, and react for 12 hours at a stirring rate of 60 rpm and room temperature to obtain precursor 1; mix butyl titanate, glacial acetic acid and anhydrous ethanol, stir at a stirring rate of 1000 rpm and room temperature, add precursor 1 and hydrochloric acid solution, stir for 40 minutes, put into an oven at a temperature of 80°C, bake for 12 hours, and then calcine at 450°C for 3 hours to obtain precursor 2;
[0043] The pH of Tris-HCl buffer is 8.5, the dosage ratio of tourmaline powder, dopamine and Tris-HCl buffer is 2g:0.007g:300mL, the mass fraction of hydrochloric acid solution is 30%, and the dosage ratio of butyl titanate, glacial acetic acid, anhydrous ethanol, precursor 1 and hydrochloric acid solution is 8mL:1.5mL:35mL:2.5g:0.4mL;
[0044] Step A2: (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide were mixed, and reacted for 3 hours at a stirring rate of 140 rpm and a temperature of 90°C under nitrogen protection to obtain azidosilane. Precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane and deionized water were mixed, and stirred at a stirring rate of 200 rpm and room temperature, and ammonia water was added to react for 2 hours. Then, azidosilane was added, and the reaction was continued for 1.5 hours. The mixture was spray-dried to obtain modified silicon microspheres.
[0045] The ratio of (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide is 3.2g:3g:60mL, the mass fraction of ammonia water is 25%, and the ratio of precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane, ammonia water and azidosilane is 6g:0.05mol:0.045mol:20mL:0.012mol;
[0046] Step A3: Modified silica microspheres, modified copolymer resin, copper sulfate and N,N-dimethylformamide were mixed, ultrasonically dispersed for 10 minutes, and under nitrogen protection, the stirring rate was 120 rpm, the temperature was 30° C., and pentamethyldiethylenetriamine was added with stirring, and the reaction was carried out for 24 hours to obtain a composite filler;
[0047] The amount ratio of modified silica microspheres, modified copolymer resin, copper sulfate and pentamethyldiethylenetriamine is 14g:15g:3.2g:12mL;
[0048] The modified copolymer resin is prepared by the following steps:
[0049] Step B1: B-trichloroborazine, trimethylsilyl acetylene magnesium chloride solution and toluene are mixed, and the mixture is reacted for 6 hours under nitrogen protection, at a stirring rate of 100 rpm and a temperature of 30°C to obtain alkynyl trichloroborazine; alkynyl trichloroborazine, methylvinyl dichlorosilane, dichlorosilane and dichloromethane are mixed, and the mixture is stirred at a stirring rate of 100 rpm and a temperature of -15°C, and ammonia is introduced, and the mixture is reacted for 4 hours to obtain modified polyborosilazane;
[0050] The molar concentration of trimethylsilyl acetylene magnesium chloride solution is 0.5 mol / L, the amount ratio of B-trichloroborazine and trimethylsilyl acetylene magnesium chloride solution is 0.065 mol:110 mL, and the amount ratio of alkynyl trichloroborazine, methylvinyl dichlorosilane and dichlorosilane is 0.03 mol:0.025 mol:0.33 mol;
[0051] Step B2: Modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, tetrahydrofuran and xylene are mixed, stirred at a stirring rate of 180 rpm and a temperature of 95° C., and 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile are added, and the mixture is reacted for 10 hours to obtain a copolymer resin, and the copolymer resin, potassium carbonate and methanol are mixed, and the mixture is reacted for 2 hours at a stirring rate of 180 rpm and room temperature to obtain a modified copolymer resin;
[0052] The amount ratio of modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile is 10g:15g:55g:20g:2g:8g, and the amount ratio of copolymer resin and potassium carbonate is 25g:16g.
[0053] Example 3 A method for preparing a fireproof and stain-resistant nano-silicon anion coating comprises the following steps: Step S1: Weigh the following raw materials in parts by weight: 60 parts of commercial Yoshida silicone acrylic emulsion, 10 parts of composite filler, 5 parts of commercial TSP-L20 nano-silicon dioxide, 1 part of commercial 7500W dispersant, 0.5 parts of commercial LKXP001 defoamer, 2 parts of commercial EPH film-forming aid, 0.5 parts of commercial TT-40 thickener and 40 parts of deionized water;
[0054] Step S2: mixing the silicone-acrylic emulsion, the composite filler, nano-silicon dioxide, the dispersant, the defoaming agent, the film-forming aid, the thickener and the deionized water, stirring for 20 minutes at a stirring rate of 1000 rpm, to prepare a fire-resistant and stain-resistant nano-silicon anion coating;
[0055] The composite filler is prepared by the following steps:
[0056] Step A1: Mix commercially available 1250 mesh tourmaline powder, dopamine and Tris-HCl buffer, ultrasonically disperse for 40 minutes, and then react for 12 hours at a stirring rate of 80 rpm and room temperature to obtain precursor 1, mix butyl titanate, glacial acetic acid and anhydrous ethanol, stir at a stirring rate of 120 rpm and room temperature, add precursor 1 and hydrochloric acid solution, stir for 40 minutes, put into an oven at a temperature of 80°C, bake for 12 hours, and then calcine at 450°C for 3 hours to obtain precursor 2;
[0057] The pH of Tris-HCl buffer is 8.5, the dosage ratio of tourmaline powder, dopamine and Tris-HCl buffer is 3 g: 0.007 g: 300 mL, the mass fraction of hydrochloric acid solution is 30%, and the dosage ratio of butyl titanate, glacial acetic acid, anhydrous ethanol, precursor 1 and hydrochloric acid solution is 10 mL: 1.5 mL: 40 mL: 2.5 g: 0.4 mL;
[0058] Step A2: (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide were mixed, and the mixture was stirred at a rate of 140 rpm and a temperature of 90°C for 4 h under nitrogen protection to obtain azidosilane. Precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane and deionized water were mixed, and ammonia water was added at a stirring rate of 200 rpm and room temperature to react for 3 h. Then azidosilane was added, and the reaction was continued for 1.5 h. The mixture was spray-dried to obtain modified silicon microspheres.
[0059] The ratio of (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide is 3.2g:3.2g:70mL, the mass fraction of ammonia water is 25%, and the ratio of precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane, ammonia water and azidosilane is 7g:0.05mol:0.055mol:24mL:0.012mol;
[0060] Step A3: Modified silica microspheres, modified copolymer resin, copper sulfate and N,N-dimethylformamide were mixed, ultrasonically dispersed for 10 minutes, and under nitrogen protection, a stirring rate of 150 rpm and a temperature of 30° C., pentamethyldiethylenetriamine was added and reacted for 24 hours to obtain a composite filler;
[0061] The amount ratio of modified silica microspheres, modified copolymer resin, copper sulfate and pentamethyldiethylenetriamine is 14g:16g:3.4g:12mL;
[0062] The modified copolymer resin is prepared by the following steps:
[0063] Step B1: B-trichloroborazine, trimethylsilyl acetylene magnesium chloride solution and toluene are mixed, and the mixture is reacted for 6 hours under nitrogen protection, at a stirring rate of 120 rpm and a temperature of 30°C to obtain alkynyl trichloroborazine; alkynyl trichloroborazine, methylvinyl dichlorosilane, dichlorosilane and dichloromethane are mixed, and the mixture is stirred at a stirring rate of 120 rpm and a temperature of -15°C, and ammonia is introduced, and the mixture is reacted for 4 hours to obtain modified polyborosilazane;
[0064] The molar concentration of trimethylsilyl acetylene magnesium chloride solution is 0.5 mol / L, the amount ratio of B-trichloroborazine and trimethylsilyl acetylene magnesium chloride solution is 0.065 mol:120 mL, and the amount ratio of alkynyl trichloroborazine, methylvinyl dichlorosilane and dichlorosilane is 0.032 mol:0.025 mol:0.35 mol;
[0065] Step B2: Modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, tetrahydrofuran and xylene are mixed, stirred at a stirring rate of 180 rpm and a temperature of 95° C., 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile are added, and the mixture is reacted for 12 hours to obtain a copolymer resin, and the copolymer resin, potassium carbonate and methanol are mixed, and the mixture is reacted for 2 hours at a stirring rate of 180 rpm and room temperature to obtain a modified copolymer resin;
[0066] The amount ratio of modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile is 12g:15g:55g:25g:3g:8g, and the amount ratio of copolymer resin and potassium carbonate is 25g:17g.
[0067] Comparative Example 1 Compared with Example 3, this comparative example replaces the azidosilane in the preparation process of the composite filler with 3-mercaptopropyltriethoxysilane, and the other steps are the same.
[0068] Comparative Example 2 Compared with Example 3, this comparative example replaces the precursor 2 in the preparation process of the composite filler with commercially available 1250 mesh tourmaline powder, and the other steps are the same.
[0069] Comparative Example 3 Compared with Example 3, this comparative example removes the acetylenic trichloroborazine in the preparation process of the modified copolymer resin, and the other steps are the same.
[0070] Comparative Example 4 Compared with Example 3, this comparative example is different in that hexafluorobutyl methacrylate in the preparation process of the modified copolymer resin is replaced by butyl methacrylate, and the other steps are the same.
[0071] Take the fire-retardant and stain-resistant nano-silicon anion coating prepared in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4, refer to GB 12441-2018, apply the nano-silicon anion coating on a 150mm×100mm×3mm steel sample, the coating thickness is 1mm, and a simulated large plate combustion test is performed, and the time taken for the surface to reach 220°C is recorded to judge its fire retardant performance, and the nano-silicon anion coating is applied on a 20cm×20cm glass plate, and the coating density is 140g / m 2 , curing for 24 hours, placing the coated glass plate in a sealed box, using a negative ion concentration tester to test the negative ion concentration, immersing the sample in a 1g / L fluorescently labeled bovine serum albumin buffer solution, soaking for 2 days, taking it out, and gently rinsing it with a buffer solution for 30 seconds, dividing the sample into 100 grids and placing it under fluorescence, calculating the percentage of the fluorescent area to the total area of the sample to determine the anti-fouling performance of the coating. The test results are shown in Table 1:
[0072] Table 1 Test results
[0073]
[0074] It can be seen from the test results in the table shown that when Example 1, Example 2 and Example 3 are compared with Comparative Example 1, Comparative Example 2, Comparative Example 3 and Comparative Example 4, Comparative Example 1 replaces the azidosilane in the preparation process of the composite filler with 3-mercaptopropyltriethoxysilane. Due to the lack of triazole groups, some of its performance is reduced. Comparative Example 2 replaces the precursor 2 in the preparation process of the composite filler with tourmaline powder. Due to the lack of titanium dioxide, its negative ion release performance is greatly reduced. Comparative Example 3 removes the acetylated trichloroborazine in the preparation process of the modified copolymer resin. Due to the lack of trichloroborazine structure, its fire resistance is greatly reduced. Comparative Example 4 replaces hexafluorobutyl methacrylate in the preparation process of the modified copolymer resin with butyl methacrylate. Due to the lack of fluorine segments, its anti-fouling performance is greatly reduced.
[0075] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0076] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a fire-resistant and stain-resistant nano-silicon anion coating, characterized in that: The method comprises the following steps: Step S1: weighing the following raw materials in parts by weight: 50-60 parts of silicone-acrylic emulsion, 8-10 parts of composite filler, 4-5 parts of nano-silicon dioxide, 0.5-1 parts of dispersant, 0.3-0.5 parts of defoamer, 1.5-2 parts of film-forming aid, 0.5 parts of thickener and 30-40 parts of deionized water; Step S2: mixing the silicone-acrylic emulsion, the composite filler, nano-silicon dioxide, the dispersant, the defoaming agent, the film-forming aid, the thickener and the deionized water, stirring for 15-20 minutes at a stirring rate of 800-1000 rpm, to prepare a fire-resistant and stain-resistant nano-silicon anion coating; The composite filler is prepared by the following steps: Step A1: Tourmaline powder, dopamine and Tris-HCl buffer were mixed, ultrasonically dispersed for 30-40 minutes, and then reacted for 12 hours at a stirring rate of 60-80 rpm and room temperature to obtain precursor 1. Butyl titanate, glacial acetic acid and anhydrous ethanol were mixed, stirred at a stirring rate of 100-120 rpm and room temperature, and precursor 1 and hydrochloric acid solution were added, stirred for 30-40 minutes, and placed in an oven at a temperature of 80° C., baked for 12 hours, and then calcined at 450° C. for 3 hours to obtain precursor 2; Step A2: (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide were mixed, and the mixture was stirred at a rate of 120-140 rpm and a temperature of 90°C for 3-4 hours under nitrogen protection to obtain azidosilane. Precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane and deionized water were mixed, and ammonia water was added at a stirring rate of 150-200 rpm and room temperature to react for 2-3 hours. Then, azidosilane was added, and the reaction was continued for 1-1.5 hours. The mixture was spray-dried to obtain modified silicon microspheres. Step A3: Modified silica microspheres, modified copolymer resin, copper sulfate and N,N-dimethylformamide are mixed, ultrasonically dispersed for 5-10 minutes, and under nitrogen protection, the stirring rate is 120-150 rpm, the temperature is 30° C., and pentamethyldiethylenetriamine is added with stirring, and the reaction is carried out for 24 hours to obtain a composite filler; The modified copolymer resin is prepared by the following steps: Step B1: B-trichloroborazine, trimethylsilyl acetylene magnesium chloride solution and toluene are mixed, and the mixture is reacted for 4-6 hours under nitrogen protection, at a stirring rate of 100-120 rpm and a temperature of 30° C. to obtain alkynyl trichloroborazine; alkynyl trichloroborazine, methylvinyl dichlorosilane, dichlorosilane and dichloromethane are mixed, and the mixture is stirred at a stirring rate of 100-120 rpm and a temperature of -15° C., and ammonia is introduced, and the mixture is reacted for 3-4 hours to obtain modified polyborosilazane; Step B2: Mix modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, tetrahydrofuran and xylene, stir and add 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile at a stirring rate of 150-180 rpm and a temperature of 95°C, and react for 10-12 hours to obtain a copolymer resin, mix the copolymer resin, potassium carbonate and methanol, and react for 1-2 hours at a stirring rate of 150-180 rpm and room temperature to obtain a modified copolymer resin.
2. The method for preparing a fire-proof and stain-resistant nano-silicon anion coating according to claim 1, characterized in that: In step A1: the pH of Tris-HCl buffer is 8.5, the dosage ratio of tourmaline powder, dopamine and Tris-HCl buffer is 2-3g: 0.006-0.007g: 300mL, the mass fraction of hydrochloric acid solution is 30%, and the dosage ratio of butyl titanate, glacial acetic acid, anhydrous ethanol, precursor 1 and hydrochloric acid solution is 8-10mL: 1-1.5mL: 35-40mL: 2-2.5g: 0.4mL.
3. The method for preparing a fire-proof and stain-resistant nano-silicon anion coating according to claim 1, characterized in that: In step A2: the ratio of (3-chloropropyl)triethoxysilane, sodium azide and N,N-dimethylformamide is 3-3.2 g: 3-3.2 g: 60-70 mL, the mass fraction of ammonia water is 25%, and the ratio of precursor 2, dimethyldimethoxysilane, phenyltrimethoxysilane, ammonia water and azidosilane is 6-7 g: 0.04-0.05 mol: 0.045-0.055 mol: 20-24 mL: 0.01-0.012 mol.
4. The method for preparing a fire-proof and stain-resistant nano-silicon anion coating according to claim 1, characterized in that: In step A3: the amount ratio of modified silica microspheres, modified copolymer resin, copper sulfate and pentamethyldiethylenetriamine is 12-14 g: 15-16 g: 3.2-3.4 g: 10-12 mL.
5. The method for preparing a fire-proof and stain-resistant nano-silicon anion coating according to claim 1, characterized in that: In step B1, the molar concentration of trimethylsilyl acetylene magnesium chloride solution is 0.5 mol / L, the amount ratio of B-trichloroborazine and trimethylsilyl acetylene magnesium chloride solution is 0.06-0.065 mol:110-120 mL, and the amount ratio of alkynyl trichloroborazine, methylvinyldichlorosilane and dichlorosilane is 0.03-0.032 mol:0.022-0.025 mol:0.33-0.35 mol.
6. The method for preparing a fire-proof and stain-resistant nano-silicon anion coating according to claim 1, characterized in that: In step B2: the amount ratio of modified polyborosilazane, acrylic acid, ethyl acrylate, hexafluorobutyl methacrylate, 2,4-diphenyl-4-methyl-1-pentene and azobisisobutyronitrile is 10-12g:15g:50-55g:20-25g:2-3g:6-8g, and the amount ratio of copolymer resin and potassium carbonate is 22-25g:16-17g.
7. A fire-resistant and stain-resistant nano-silicon anion coating, characterized in that: Prepared according to any one of claims 1 to 6.