A heat-resistant and salt-resistant gel dispersion type flooding agent and preparation method thereof

By introducing multiple crosslinking network structures into frozen glues, the combination of P (AM-AMPS) copolymer, phenolic resin and cationic amide cellulose is solved, and the problem of poor heat resistance of traditional frozen glues in high-temperature and high-salt environments is solved. , achieving higher glue-forming strength and viscosity retention, and is suitable for frozen rubber-regulating and water-blocking technology in high-salt oil fields.

CN118580844BActive Publication Date: 2024-11-01DONGYING HONGCHUANG PETROLEUM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076223.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-01
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Traditional acrylamide polymer frozen gel mixing agents have poor heat resistance in high temperature and high salt environments and poor glue-forming performance, which cannot effectively solve the problem of high water content and water blocking effect in oil wells.

Method used

Using the P (AM-AMPS) copolymer, phenolic resin crosslinking agent and cationic amidated cellulose, the phenolic resin reacts with amide bonds in the copolymer and amide bonds of cationic amidated cellulose to form Multiple cross-linking network improves the glue-forming strength and viscosity retention rate of frozen glue.

Benefits of technology

It significantly improves the stability and high temperature resistance of frozen glue, shows excellent salt resistance and sealing effect, maintains good glue-forming strength and viscosity in high-temperature and high-salt environments, and meets the control of frozen glue and water blocking. Practical application requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The present invention belongs to the technical field of oilfield chemistry, and discloses a heat-resistant and salt-resistant jelly dispersion type displacement agent and a preparation method. The displacement agent includes a copolymer of 6-13 parts by weight of acrylamide and 2-acrylamide-2-methylpropanesulfonate sodium, 4-9 parts by weight of phenolic resin crosslinking agent, and 0.5-3 parts by weight of cationic amidated cellulose; in the process of forming jelly, the phenolic resin crosslinking agent and the amide bond in the copolymer form a first crosslinking network, the amide bond of the phenolic resin crosslinking agent and the cationic amidated cellulose and the second crosslinking network, and at the same time, the sodium sulfonate salt in the copolymer and the quaternary ammonium salt cation of the cationic amidated cellulose interact electrostatically to form a third crosslinking network; the jelly displacement agent has good gel strength and viscosity retention rate, and has excellent salt resistance and temperature resistance; it can meet the displacement technology and construction of the jelly displacement agent in high-salt and high-temperature oil fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oilfield chemistry, in particular to a temperature-resistant and salt-resistant gel dispersion type displacement agent and a preparation method thereof. Background Art

[0002] In the process of oil field development, water is injected into the reservoir through injection wells to maintain or restore the oil layer pressure, thereby increasing the driving force of the reservoir and improving the production speed and recovery rate of the reservoir. However, with the continuous development of water injection, the water content in the oil wells gradually increases, resulting in violent flooding and well wall instability in the oil wells, affecting the recovery rate of the reservoir and posing safety hazards in operations. Using cement plugging agents, polymer gels, and gels for flooding and water plugging is an effective way to solve the problem of high water content in oil reservoirs.

[0003] At present, the gel-adjusting and displacing agent is mainly a gel-adjusting and displacing system formed by acrylamide polymers and phenolic resins, which uses the hydroxymethyl of phenolic resins to cross-link with the amide bonds of acrylamide polymers to form a cross-linked network gel, which has good displacing and water plugging effects. However, the traditional acrylamide polymer gel-adjusting and displacing agent has the problem of poor heat resistance, and the gelling performance is not good in harsh oil reservoir exploitation environments such as high temperature and high salt. The patent of publication number CN117683529A discloses a preparation method of a double cross-linked polyacrylamide gel fracturing fluid, which adopts a mixed double cross-linking system of inorganic boron and phenolic resin, forms a body-shaped micro-cross-linked network structure in the polyacrylamide fracturing system, and improves the stability of the fracturing system in a high temperature and high salt environment. However, the gel fracturing fluid does not show good water plugging and plugging performance, which is not conducive to the practical application in gel-adjusting and water plugging. Summary of the invention

[0004] The invention solves the problem that the jelly dispersion type control and displacement agent has poor temperature resistance and salt resistance.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is: a temperature-resistant and salt-resistant jelly dispersion type control agent, comprising the following raw materials: 6-13 parts by weight of P (AM-AMPS) copolymer, 4-9 parts by weight of phenolic resin crosslinking agent, and 0.5-3 parts by weight of cationic amidated cellulose.

[0006] Among them, P (AM-AMPS) copolymer is a copolymer of acrylamide and sodium 2-acrylamido-2-methylpropane sulfonate.

[0007] The preparation method of cationic amidated cellulose is as follows: add dimethyl sulfoxide and carboxymethyl cellulose into a reaction bottle, stir and mix, then add N,N'-dicyclohexylcarbodiimide and 4-dimethylaminopyridine, stir and activate, then add a cationic amide modifier, stir and react, add ethanol for precipitation, filter and wash with ethanol, dry, and obtain cationic amidated cellulose.

[0008] The cationic amide modifier has the structural formula (I) shown below.

[0009] Formula (I).

[0010] The masses of N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and cationic amide modifier are 22-146%, 6-40% and 30-200% of the mass of carboxymethyl cellulose respectively.

[0011] The activation temperature is 20-35°C, the time is 2-4h, and the reaction time is 24-48h.

[0012] The preparation method of the cationic amide modifier is as follows: add sodium hydroxide aqueous solution, 2,3-epoxypropyltrimethylammonium chloride and 4-hydroxybenzamide with a mass concentration of (3-6) g / L into a reaction bottle, heat to 55-70°C, stir and react for 2-4 hours, add hydrochloric acid solution to neutralize the solution to pH 7, add saturated sodium chloride solution and ethyl acetate, oscillate and extract, separate, combine the organic phases, dry and remove water with anhydrous sodium sulfate, filter, rotary evaporate the filtrate, add ethanol for recrystallization, and obtain the cationic amide modifier.

[0013] Among them, the mass of 2,3-epoxypropyltrimethylammonium chloride is 125-160% of the mass of 4-hydroxybenzamide.

[0014] The preparation method of the P (AM-AMPS) copolymer is as follows: water, acrylamide, sodium 2-acrylamido-2-methylpropane sulfonate, ammonium persulfate and sodium bisulfite are added into a reaction bottle, nitrogen is introduced to carry out a polymerization reaction, freeze-drying after the reaction, washing with acetone and drying to obtain the P (AM-AMPS) copolymer.

[0015] The preparation method of the temperature-resistant and salt-resistant jelly dispersion type control agent comprises the steps of weighing raw materials and stirring and mixing the raw materials.

[0016] The technical effect of the present invention is as follows: the present invention reacts 2,3-epoxypropyltrimethylammonium chloride and 4-hydroxybenzamide to obtain a cationic amide modifier, and then uses N,N'-dicyclohexylcarbodiimide and 4-dimethylaminopyridine as catalysts to esterify the cationic amide modifier with carboxymethyl cellulose to obtain cationic amidated cellulose, thereby introducing quaternary ammonium salt cations and amide bonds ( ).

[0017] The invention uses a copolymer of acrylamide and sodium 2-acrylamido-2-methylpropane sulfonate as the polymer main agent of the jelly adjusting and displacing agent, a phenolic resin as a crosslinking agent, and a cationic amidated cellulose as an auxiliary crosslinking agent. In the process of forming the jelly, the hydroxymethyl of the phenolic resin crosslinking agent reacts with the amide bond in the acrylamide copolymer to form a first crosslinking network, the hydroxymethyl of the phenolic resin crosslinking agent reacts with the amide bond of the cationic amidated cellulose to form a second crosslinking network, and at the same time, the sodium sulfonic acid salt in the copolymer and the quaternary ammonium salt cation of the cationic amidated cellulose form a third crosslinking network through electrostatic interaction. Through multiple crosslinking effects, the gelling process of the jelly adjusting and displacing agent is accelerated, which is beneficial to reducing the gelling time; and the multiple crosslinking networks formed at the same time significantly improve the gelling strength and viscosity retention rate of the jelly adjusting and displacing agent, and show better jelly stability. Moreover, in the low mineralization system of 10007mg / L and the high mineralization system of 29984mg / L, the gelling agent has good gelling strength and viscosity retention rate, and has excellent salt resistance, which can meet the requirements of gelling agent in the flooding technology and construction in high-salt oil fields.

[0018] The gel displacement agent of the present invention has a multi-crosslinked stable gel structure and strong high temperature resistance. After the plugging performance test, the gel is not easy to decompose at high temperature, and has a high plugging rate in high temperature systems of 90°C and 150°C. It shows good temperature resistance and plugging performance. It can meet the needs of gel displacement agent in gel profile control and water plugging technology in high-salinity oil reservoirs. DETAILED DESCRIPTION

[0019] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in the art or the product instructions are used.

[0020] Example 1

[0021] (1) Add 30 mL of 6 g / L sodium hydroxide aqueous solution, 5.8 g of 2,3-epoxypropyltrimethylammonium chloride, and 4 g of 4-hydroxybenzamide to the reaction bottle, heat to 70°C, stir and react for 2 h, add hydrochloric acid solution to neutralize the solution to pH 7, add saturated sodium chloride solution and ethyl acetate, oscillate and extract, separate, combine the organic phases, dry with anhydrous sodium sulfate to remove water, filter, rotary evaporate the filtrate, add ethanol for recrystallization, and obtain a cationic amide modifier. The reaction formula is:

[0022]

[0023] (2) Add 100 mL of dimethyl sulfoxide and 5 g of carboxymethyl cellulose to the reaction bottle, stir and mix, then add 7.3 g of N,N'-dicyclohexylcarbodiimide and 2 g of 4-dimethylaminopyridine, stir and activate at 30°C for 4 h, then add 10 g of cationic amide modifier, stir and react for 48 h, add ethanol for precipitation, filter, wash with ethanol, and dry to obtain cationic amidated cellulose. The reaction formula is:

[0024]

[0025] (3) Add 600 mL of water, 80 g of acrylamide, 20 g of sodium 2-acrylamido-2-methylpropane sulfonate, 0.18 g of ammonium persulfate, and 0.18 g of sodium bisulfite into a reaction flask, introduce nitrogen, and react at 45 °C for 3 h. After the reaction, freeze-dry, wash with acetone, and dry to obtain P (AM-AMPS) copolymer.

[0026] (4) Add 1L of distilled water, calcium chloride, sodium chloride, magnesium chloride, sodium sulfate, sodium bicarbonate, sodium carbonate and potassium chloride into a container to prepare simulated formation water with different mineralizations; then add 6g of P (AM-AMPS) copolymer, 4g of phenolic resin crosslinking agent and 0.5g of cationic amidated cellulose, stir and mix well to obtain a temperature-resistant and salt-resistant gel dispersion type displacement agent.

[0027] Example 2

[0028] (1) Add 40 mL of 3 g / L sodium hydroxide aqueous solution, 6.4 g of 2,3-epoxypropyltrimethylammonium chloride, and 4 g of 4-hydroxybenzamide to a reaction bottle, heat to 55 °C, stir and react for 4 h, add hydrochloric acid solution to neutralize the solution to pH 7, add saturated sodium chloride solution and ethyl acetate, oscillate and extract, separate, combine the organic phases, dry with anhydrous sodium sulfate to remove water, filter, rotary evaporate the filtrate, add ethanol to recrystallize, and obtain a cationic amide modifier.

[0029] (2) Add 80 mL of dimethyl sulfoxide and 5 g of carboxymethyl cellulose to the reaction bottle, stir and mix, then add 4.3 g of N,N'-dicyclohexylcarbodiimide and 1.2 g of 4-dimethylaminopyridine, stir and activate at 20°C for 4 h, then add 6 g of cationic amide modifier, stir and react for 48 h, add ethanol for precipitation, filter, wash with ethanol, and dry to obtain cationic amidated cellulose.

[0030] (3) Add 600 mL of water, 75 g of acrylamide, 25 g of sodium 2-acrylamido-2-methylpropanesulfonate, 0.2 g of ammonium persulfate, and 0.2 g of sodium bisulfite into a reaction bottle, introduce nitrogen, and react at 50 °C for 3 h. After the reaction, freeze-dry, wash with acetone, and dry to obtain P (AM-AMPS) copolymer.

[0031] (4) Add 1L of distilled water, calcium chloride, sodium chloride, magnesium chloride, sodium sulfate, sodium bicarbonate, sodium carbonate and potassium chloride into a container to prepare simulated formation water with different mineralizations; then add 8.5g of P (AM-AMPS) copolymer, 5.8g of phenolic resin cross-linking agent and 1.3g of cationic amidated cellulose, stir and mix well to obtain a temperature-resistant and salt-resistant gel dispersion type displacement agent.

[0032] Example 3

[0033] (1) Add 40 mL of 4.5 g / L sodium hydroxide aqueous solution, 5 g of 2,3-epoxypropyltrimethylammonium chloride, and 4 g of 4-hydroxybenzamide to a reaction bottle, heat to 70°C, stir and react for 3 h, add hydrochloric acid solution to neutralize the solution to pH 7, add saturated sodium chloride solution and ethyl acetate, oscillate and extract, separate, combine the organic phases, dry with anhydrous sodium sulfate to remove water, filter, rotary evaporate the filtrate, add ethanol to recrystallize, and obtain a cationic amide modifier.

[0034] (2) Add 50 mL of dimethyl sulfoxide and 5 g of carboxymethyl cellulose to the reaction bottle, stir and mix, then add 1.1 g of N,N'-dicyclohexylcarbodiimide and 0.3 g of 4-dimethylaminopyridine, stir and activate at 35°C for 2 h, then add 1.5 g of cationic amide modifier, stir and react for 36 h, add ethanol for precipitation, filter, wash with ethanol, and dry to obtain cationic amidated cellulose.

[0035] (3) Add 600 mL of water, 75 g of acrylamide, 25 g of sodium 2-acrylamido-2-methylpropanesulfonate, 0.2 g of ammonium persulfate, and 0.2 g of sodium bisulfite into the reaction bottle, introduce nitrogen, and react at 40 °C for 4 h. After the reaction, freeze-dry, wash with acetone, and dry to obtain P (AM-AMPS) copolymer.

[0036] (4) Add 1L of distilled water, calcium chloride, sodium chloride, magnesium chloride, sodium sulfate, sodium bicarbonate, sodium carbonate and potassium chloride into a container to prepare simulated formation water with different mineralizations; then add 11g of P (AM-AMPS) copolymer, 7.4g of phenolic resin cross-linking agent and 2.2g of cationic amidated cellulose, stir and mix well to obtain a temperature-resistant and salt-resistant gel dispersion type displacement agent.

[0037] Example 4

[0038] (1) Add 40 mL of 4 g / L sodium hydroxide aqueous solution, 5 g of 2,3-epoxypropyltrimethylammonium chloride, and 4 g of 4-hydroxybenzamide to a reaction bottle, heat to 70°C, stir and react for 3 h, add hydrochloric acid solution to neutralize the solution to pH 7, add saturated sodium chloride solution and ethyl acetate, oscillate and extract, separate, combine the organic phases, dry with anhydrous sodium sulfate to remove water, filter, rotary evaporate the filtrate, add ethanol to recrystallize, and obtain a cationic amide modifier.

[0039] (2) Add 50 mL of dimethyl sulfoxide and 5 g of carboxymethyl cellulose to the reaction bottle, stir and mix, then add 1.1 g of N,N'-dicyclohexylcarbodiimide and 0.3 g of 4-dimethylaminopyridine, stir and activate at 35°C for 2 h, then add 1.5 g of cationic amide modifier, stir and react for 24 h, add ethanol for precipitation, filter, wash with ethanol, and dry to obtain cationic amidated cellulose.

[0040] (3) Add 600 mL of water, 70 g of acrylamide, 30 g of sodium 2-acrylamido-2-methylpropanesulfonate, 0.2 g of ammonium persulfate, and 0.2 g of sodium bisulfite into a reaction bottle, introduce nitrogen, and react at 40 °C for 4 h. After the reaction, freeze-dry, wash with acetone, and dry to obtain P (AM-AMPS) copolymer.

[0041] (4) Add 1L of distilled water, calcium chloride, sodium chloride, magnesium chloride, sodium sulfate, sodium bicarbonate, sodium carbonate and potassium chloride into a container to prepare simulated formation water with different mineralizations; then add 13g of P (AM-AMPS) copolymer, 9g of phenolic resin crosslinker and 3g of cationic amidated cellulose, stir and mix well to obtain a temperature-resistant and salt-resistant gel dispersion type displacement agent.

[0042] Comparative Example 1

[0043] (1) Add 1L of distilled water, calcium chloride, sodium chloride, magnesium chloride, sodium sulfate, sodium bicarbonate, sodium carbonate and potassium chloride into a container to prepare simulated formation water with different mineralizations; then add 6g of P (AM-AMPS) copolymer (prepared in the same manner as in Example 1) and 4g of phenolic resin cross-linking agent, stir and mix to obtain a gel dispersion type displacement agent.

[0044] Comparative Example 2

[0045] (1) Add 1L of distilled water, calcium chloride, sodium chloride, magnesium chloride, sodium sulfate, sodium bicarbonate, sodium carbonate and potassium chloride into a container to prepare simulated formation water with different mineralizations; then add 6g of P (AM-AMPS) copolymer (prepared in the same manner as in Example 1), 4g of phenolic resin cross-linking agent and 0.5g of carboxymethyl cellulose, stir and mix to obtain a jelly dispersion type displacement agent.

[0046] Comparative Example 3

[0047] (1) Add 100 mL of dimethyl sulfoxide and 5 g of microcrystalline cellulose to a reaction bottle, stir and mix, then add 0.15 g of sodium hydroxide, heat to 65°C, add 10 g of 2,3-epoxypropyltrimethylammonium chloride, react for 6 hours, add ethanol for precipitation, filter, wash with ethanol, and dry to obtain cationic cellulose. The reaction formula is:

[0048]

[0049] (2) Add 1L of distilled water, calcium chloride, sodium chloride, magnesium chloride, sodium sulfate, sodium bicarbonate, sodium carbonate and potassium chloride into a container to prepare simulated formation water with different mineralizations; then add 6g of P (AM-AMPS) copolymer, 4g of phenolic resin crosslinking agent and 0.5g of cationic cellulose, stir and mix well to obtain a gel dispersion type displacement agent.

[0050] The mineralization of the simulated formation water was controlled to be 10007 and 29984 mg / L, and the gel dispersion type displacement agent was placed in an oven and gelled at 90°C. The viscosity value was measured by a viscometer every 2 hours. When the viscosity remained unchanged, the gelling time was the gelling time, and the maximum viscosity value P1 was recorded. The viscosity value was the gelling strength. After 6 months of gelling, the viscosity value P2 was measured again, and the viscosity retention rate W was calculated, W=P2 / P1×100%. The greater the viscosity retention rate, the better the gel stability.

[0051] Table 1 Gelation performance test when the simulated formation water mineralization is 10007 mg / L

[0052]

[0053] Table 2 Gelation performance test when the simulated formation water mineralization is 29984 mg / L

[0054]

[0055] Fill the core with 50 mesh quartz sand; use water flooding method to test the permeability A1 of the core before plugging; then inject 0.3PV of gel dispersion type displacement agent into the core, and the simulated formation water salinity in the displacement agent is 10007mg / L; then place the core in an oven, set the gelling temperature to 90-150℃, continue water flooding after gelling for 48 hours, test the permeability A2 after plugging, and calculate the plugging rate R. R=(A1-A2) / A1×100%, the larger the plugging rate, the better the displacement and plugging performance.

[0056] Table 3 Plugging performance test at gelling temperature of 90°C

[0057]

[0058] Table 4 Plugging performance test at gelling temperature of 150°C

[0059]

[0060] The above description of the embodiments is to facilitate those of ordinary skill in the art to understand and apply the present application. It is obvious that those familiar with the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without having to pay creative labor. Therefore, the present application is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the contents disclosed in the present application without departing from the scope and spirit of the present application are within the scope of the present application.

Claims

1. A heat-resistant and salt-resistant gel dispersion type flooding agent, It is characterized in that The heat-resistant and salt-resistant gel dispersion type control agent comprises the following raw materials: 6-13 parts by weight of P (AM-AMPS) copolymer, 4-9 parts by weight of phenolic resin crosslinking agent and 0.5-3 parts by weight of cationic amidated cellulose; The P (AM-AMPS) copolymer is a copolymer of acrylamide and sodium 2-acrylamido-2-methylpropane sulfonate; The preparation method of the cationic amidated cellulose comprises: adding dimethyl sulfoxide and carboxymethyl cellulose into a reaction bottle, stirring and mixing, then adding N,N'-dicyclohexylcarbodiimide and 4-dimethylaminopyridine, stirring and activating, then adding a cationic amide modifier, stirring and reacting, precipitating, filtering, washing, and drying to obtain the cationic amidated cellulose; The cationic amide modifier has the structural formula (I) as follows: Formula (I).

2. The heat-resistant and salt-resistant jelly dispersion type displacement agent according to claim 1, It is characterized in that The masses of the N,N'-dicyclohexylcarbodiimide, 4-dimethylaminopyridine and cationic amide modifier are 22-146%, 6-40% and 30-200% of the mass of the carboxymethyl cellulose respectively.

3. The heat-resistant and salt-resistant jelly dispersion type displacement agent according to claim 1, It is characterized in that The activation temperature is 20-35°C, the time is 2-4h; the reaction time is 24-48h.

4. The heat-resistant and salt-resistant jelly dispersion type displacement agent according to claim 1, It is characterized in that The preparation method of the cationic amide modifier comprises the following steps: adding sodium hydroxide aqueous solution, 2,3-epoxypropyltrimethylammonium chloride and 4-hydroxybenzamide into a reaction bottle, stirring for reaction, adding hydrochloric acid solution for neutralization, extracting and separating, and recrystallizing to obtain the cationic amide modifier.

5. The heat-resistant and salt-resistant jelly dispersion type displacement agent according to claim 4, It is characterized in that The mass concentration of the sodium hydroxide aqueous solution is (3-6) g / L.

6. The heat-resistant and salt-resistant jelly dispersion type displacement agent according to claim 4, It is characterized in that The mass of the 2,3-epoxypropyltrimethylammonium chloride is 125-160% of the mass of 4-hydroxybenzamide.

7. The heat-resistant and salt-resistant jelly dispersion type displacement agent according to claim 4, It is characterized in that In the preparation method of the cationic amide modifier, the reaction temperature is 55-70° C. and the reaction time is 2-4 hours.

8. The heat-resistant and salt-resistant jelly dispersion type displacement agent according to claim 1, It is characterized in that The preparation method of the P (AM-AMPS) copolymer comprises the following steps: adding water, acrylamide, sodium 2-acrylamido-2-methylpropanesulfonate, ammonium persulfate and sodium bisulfite into a reaction bottle, introducing nitrogen gas to carry out polymerization reaction, freeze-drying after the reaction, washing with acetone and drying to obtain the P (AM-AMPS) copolymer.

9. A method for preparing the temperature-resistant and salt-resistant jelly dispersion type displacement agent according to any one of claims 1 to 8, It is characterized in that The method comprises the steps of weighing raw materials and stirring and mixing the raw materials.