A kind of high sweat absorption color spinning yarn and preparation method thereof

By introducing a copolymerization and stretching process of modifiers and polyester raw materials, the problem of insufficient sweat absorption performance of polyester fibers is solved, and high water absorption and rapid drying and color fastness are improved, which is suitable for clothing materials.

CN118581593BActive Publication Date: 2024-11-12高创(盐城)技术转移有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410834251.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-11-12
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Polyester fibers lack sweat-absorbing properties. The prior art changes the cross-sectional shape of the fiber or blends the pore-forming materials, resulting in complex molding processes and uncontrolled mechanical properties, making it difficult to achieve good moisture-absorbing and sweat-absorbing functions.

Method used

By introducing a modifier to copolymerize with polyester raw material and combining with the stretching process, a highly sweat-absorbing color spinning is prepared. The modifier forms amino-terminated oligomerization through amine ester exchange, epoxidation intermediate ring opening and polyetheramine reaction to form amino-terminated oligomerization It can enhance the hydrophilicity and specific surface area of ​​the fiber, and form fine cracks in the micro-nano structure to improve water absorption performance.

Benefits of technology

It realizes the rapid water absorption and quick drying properties of polyester fibers, while improving color fastness, and is suitable for clothing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004912706780000021
    Figure BDA0004912706780000021
  • Figure BDA0004912706780000031
    Figure BDA0004912706780000031
  • Figure BDA0004912706780000032
    Figure BDA0004912706780000032
Patent Text Reader

Abstract

The invention relates to a high-sweat absorption colored spun yarn and a preparation method thereof, and belongs to the technical field of polyester fibers. The colored spun yarn is based on polyester, and a modifier is introduced to copolymerize with a polyester raw material, and a stretching process is used to give the colored spun yarn fiber good moisture absorption and quick-drying performance. The modifier introduces a polyether segment into the main chain of the polymer chain to improve the hydrophilicity of the polymer, and introduces a poly-fluorine structure into the side chain of the polymer chain to produce a segregation effect in the colored spun yarn fiber. During the stretching process, the fluorine structure is used as the original defect to produce a large number of fine cracks with micro-nano structures. These fine cracks form a capillary effect, and the improvement of the hydrophilicity by the polyether segment enables the colored spun yarn fiber to absorb water quickly. The fine cracks also increase the specific surface area of ​​the colored spun yarn fiber, which is conducive to the rapid evaporation of water. It has good sweat absorption and quick-drying effect when applied to clothing materials. At the same time, these fine cracks are easier to store dyes during the dyeing process, so that the colored spun yarn has excellent color fastness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polyester fibers, and in particular relates to a high-sweat absorption colored spun yarn and a preparation method thereof. Background Art

[0002] As people have higher and higher requirements for the comfort, health, safety and environmental protection of clothing fabrics, the trend of mutual penetration and integration of casual wear and sportswear is increasingly favored by consumers. The fabrics of this kind of clothing are required to be comfortable and not stick to the skin and cause discomfort when sweating during activities. Therefore, new requirements are put forward for the moisture absorption and perspiration function of the fabric fibers.

[0003] Polyester fiber is a polymer fiber material made by polycondensation of terephthalic acid and ethylene glycol. It has the advantages of high strength, good stiffness and low cost and is widely used in clothing textiles. However, polyester materials lack hydrophilic groups and have a high degree of regularity in molecular structure, making them difficult to absorb sweat. At present, the production of moisture wicking fibers mainly adopts two technical means. First, various fibers with non-circular cross-sectional shapes are manufactured by changing the spinneret hole shape and spinning process conditions during the processing. By changing the cross-sectional shape of the fiber, the gap between the single fibers is increased, and the increase in specific surface area and capillary effect greatly improve the moisture conductivity. For example, the existing "cross" and "H" cross-sectional fibers increase the moisture conductivity of the fibers to a certain extent, but the molding process of the fibers is complicated, and excessive increase in cross-sectional area increases the molding difficulty, and broken fibers are prone to occur during the spinning process. Second, by blending and adding pore-forming materials, dissolving or etching in the subsequent processing process, pores are formed on the fiber surface to increase the specific surface area. This type of method has a complicated molding process, and the pore-forming materials are not easy to disperse, resulting in uncontrolled mechanical properties of the fibers. Summary of the invention

[0004] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a high sweat-absorbent colored spun yarn and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A high sweat-absorbent colored spun yarn is prepared by spinning, stretching and dyeing modified polyester, wherein the modified polyester is prepared by the following method:

[0007] Step A1: diethanolamine, methyl trifluoroacetate and anhydrous tetrahydrofuran are mixed, and dry nitrogen is introduced for protection. The temperature is controlled at 10-20°C in an ice-water bath, and stirring is applied at 120-150rpm. Sodium hydride is added in batches and the adding time is controlled to be 1.2-1.8h. Then the temperature is raised to 40±2°C and reflux reaction is continued for 4-5h. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water, the aqueous phase is removed and vacuum dried to obtain a fluorinated matrix;

[0008] In the above reaction, the dosage ratio of diethanolamine, methyl trifluoroacetate, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.1 mol: 0.36-0.42 g: 35-45 mL. Under the promotion of sodium hydride, diethanolamine and methyl trifluoroacetate undergo amine ester exchange. The specific reaction route is shown as follows:

[0009]

[0010] Step A2: Mix the fluorinated substrate, epichlorohydrin and dioxane, introduce nitrogen protection, heat to 75-85°C, stir at 60-90rpm for 40-60min, then cool to 30-40°C, slowly add sodium hydroxide aqueous solution, continue to stir at constant temperature after complete addition, control the total reaction time of adding sodium hydroxide aqueous solution to be 2.5-3.5h, filter after the reaction is completed, add water to the filtrate, wash and separate, remove the aqueous phase and vacuum dry to obtain an epoxidation intermediate;

[0011] In the above reaction, the amount ratio of the fluorinated substrate, epichlorohydrin, sodium hydroxide and dioxane is 0.1 mol: 0.207-0.212 mol: 3.5-4 g: 60-75 mL. Epichlorohydrin and the fluorinated substrate are ring-opened and then ring-closed under alkaline conditions. The specific reaction route is shown as follows:

[0012]

[0013] Step A3: Mix the polyetheramine and anhydrous ethanol, control the temperature in an ice-water bath to no higher than 5°C, add the epoxidation intermediate under ultrasonic vibration, control the reaction time to be 1-1.3h, and evaporate the ethanol under reduced pressure after the reaction to obtain a modifier;

[0014] In the above reaction, the ratio of the epoxidation intermediate, the amino content of the polyetheramine and the anhydrous ethanol is 0.1 mol: 0.22-0.23 mol: 50-70 mL. The epoxidation intermediate and the excess polyetheramine are ring-opened at low temperature to form an amino-terminated oligomer containing a polyether segment. The specific reaction route is shown as follows:

[0015]

[0016] Step A4: terephthalic acid, ethylene glycol, a modifier and ethylene glycol antimony are mixed, nitrogen is introduced for protection, the temperature is raised to 160-180°C for esterification for 1.5-2h, then the pressure is reduced to 100Pa, the temperature is further raised to 220-240°C, polycondensation is performed for 1-1.2h, and after the reaction is completed, the material is discharged, cooled and pelletized under nitrogen protection to obtain a modified polyester;

[0017] In the above reaction, the usage ratio of terephthalic acid, ethylene glycol, modifier and ethylene glycol antimony is 1 mol: 1.2-1.35 mol: 40-50 g: 0.1-0.12 g, and terephthalic acid, ethylene glycol and modifier are randomly copolymerized to form a copolyester of modifier blocks.

[0018] A method for preparing high sweat-absorbing colored spun yarn comprises the following steps:

[0019] Step S1: melt spinning the modified polyester, cooling and shaping it, and winding it to obtain modified filaments;

[0020] Step S2: thermally stretching the modified filaments with double rollers, cooling and winding the filaments to obtain stretched filaments;

[0021] Step S3: The stretched filaments are twice dipped and twice rolled in dye solution for coloring, and then rinsed to remove floating color and then dried to obtain highly sweat-absorbent colored spun yarn.

[0022] Furthermore, during the melt spinning process, the temperature of the spinning box is 300±10°C.

[0023] Furthermore, the stretching ratio of the double-roller heat stretching is 2.2-2.5.

[0024] Beneficial effects of the present invention:

[0025] The invention discloses a polyester-based colored spinning yarn. The colored spinning yarn fiber is endowed with good moisture absorption and quick-drying performance by introducing a modifier to copolymerize with a polyester raw material and cooperating with a stretching process. The modifier is prepared by amine ester exchange of diethanolamine and methyl trifluoroacetate to form a fluorine-containing diol compound, i.e., a fluorinated matrix. Then, epichlorohydrin and the terminal alcohol hydroxyl group of the fluorinated matrix are ring-opened and closed to introduce a terminal epoxy group for modification, i.e., an epoxidized intermediate. Then, the epoxidized intermediate and an excess of polyetheramine are ring-opened at low temperature to form an amino-terminated oligomer containing a polyether chain segment, i.e., to obtain the modifier. The modifier is copolymerized with phthalic acid and ethylene glycol to introduce a polyether chain segment into the main chain of the polymer chain to enhance the polymer chain. In order to improve the hydrophilicity of the material, the modifier introduces a polyfluorine structure into the side chain of the polymer chain. The fluorine structure is not compatible with the polyester chain, which produces a segregation effect in the colored spun yarn fiber. During the stretching process, the fluorine structure is used as the original defect to produce a large number of fine cracks with micro-nano structure. These fine cracks form capillary action, and the improvement of the hydrophilicity of the polyether segment makes the colored spun yarn fiber absorb water quickly. The fine cracks also increase the specific surface area of ​​the colored spun yarn fiber, which is beneficial to the rapid evaporation of water. It has good sweat absorption and quick-drying effect when used in clothing materials. At the same time, these fine cracks are easier to store dyes during the dyeing process, which makes the colored spun yarn have excellent color fastness. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1, preparation of high sweat absorption colored spun yarn, the specific implementation process is as follows:

[0028] (1) Preparation of modified polyester

[0029] Step A1: diethanolamine, methyl trifluoroacetate and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is controlled at 10°C in an ice-water bath, stirring is applied at 120rpm, equal amounts of sodium hydride are added in three batches, and the addition time is controlled to be 1.8h. After complete addition, the temperature is raised to 40±2°C and the reflux reaction is continued for 5h, wherein the amount ratio of diethanolamine, methyl trifluoroacetate, sodium hydride and anhydrous tetrahydrofuran is 0.1mol:0.1mol:0.36g:35mL. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water, the aqueous phase is removed and vacuum dried to obtain a fluorinated matrix.

[0030] Step A2: Take a fluorinated substrate, epichlorohydrin and dioxane, mix them, pass nitrogen protection, heat to 75°C, apply 60rpm stirring to react for 60min, then cool to 30°C, prepare a saturated aqueous solution of sodium hydroxide, slowly add the aqueous solution of sodium hydroxide, the addition time is 1.5h, continue the constant temperature reaction after complete addition, and control the total reaction time of the sodium hydroxide solution to be 3.5h, wherein the amount ratio of the fluorinated substrate, epichlorohydrin, sodium hydroxide and dioxane is 0.1mol:0.207mol:3.5g:60mL. After the reaction is completed, filter, add water to the filtrate, wash and separate, remove the aqueous phase and vacuum dry to obtain an epoxidation intermediate.

[0031] Step A3: Mix polyetheramine and anhydrous ethanol. During the implementation process, polyetheramine D230 is used. The temperature is controlled not higher than 5°C in an ice-water bath. Ultrasonic vibration of 25kHz is applied. The epoxidation intermediate is added to react for 1.3h. The ratio of the epoxidation intermediate, the amino content of the polyetheramine and the anhydrous ethanol is 0.1mol:0.22mol:50mL. After the reaction is completed, the ethanol is evaporated under reduced pressure to obtain a modifier.

[0032] Step A4: terephthalic acid, ethylene glycol, modifier and ethylene glycol antimony are mixed, nitrogen is introduced for protection, the temperature is raised to 160°C for esterification for 2 hours, and then the pressure is reduced to 100 Pa, and the temperature is continued to be raised to 220°C for condensation for 1.2 hours, wherein the amount ratio of terephthalic acid, ethylene glycol, modifier and ethylene glycol antimony is 1 mol: 1.35 mol: 40 g: 0.12 g. After the reaction is completed, the material is discharged, cooled and pelletized under nitrogen protection to obtain modified polyester.

[0033] (2) Preparation of colored yarn

[0034] Step S1: adding the modified polyester into the spinning machine, controlling the temperature of the spinning box to 300±10°C, melt-spinning the modified polyester, cooling it with side-blowing air at a wind temperature of 25°C, cooling and shaping the molten filaments, and winding them to obtain modified filaments.

[0035] Step S2: heat-stretching the modified filaments with two rollers, with the temperature of roller 1 being 95±2°C and the temperature of roller 2 being 125±5°C, controlling the stretching multiple to be 2.2, and cooling and winding to obtain stretched filaments.

[0036] Step S3: The stretched filaments are twice dipped and twice rolled in dye solution for coloring, and then rinsed to remove floating color and then dried to obtain highly sweat-absorbent colored spun yarn.

[0037] Example 2, preparation of high sweat absorption colored spun yarn, the specific implementation process is as follows:

[0038] (1) Preparation of modified polyester

[0039] Step A1: diethanolamine, methyl trifluoroacetate and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is controlled at 20°C in an ice-water bath, stirring is applied at 150 rpm, equal amounts of sodium hydride are added in three batches, and the addition time is controlled to be 1.2 h. After complete addition, the temperature is raised to 40±2°C and reflux reaction is continued for 4 h, wherein the amount ratio of diethanolamine, methyl trifluoroacetate, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.1 mol: 0.42 g: 45 mL. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water, the aqueous phase is removed and vacuum dried to obtain a fluorinated matrix.

[0040] Step A2: Take a fluorinated substrate, epichlorohydrin and dioxane, mix them, pass nitrogen protection, heat to 85°C, apply 90rpm stirring to react for 40 minutes, then cool to 40°C, prepare a saturated aqueous solution of sodium hydroxide, slowly add the aqueous solution of sodium hydroxide, the addition time is 1 hour, continue the constant temperature reaction after complete addition, and control the total reaction time of the sodium hydroxide solution to be 2.5 hours, wherein the amount ratio of the fluorinated substrate, epichlorohydrin, sodium hydroxide and dioxane is 0.1 mol: 0.212 mol: 4 g: 75 mL. After the reaction is completed, filter, add water to the filtrate, wash and separate, remove the aqueous phase and vacuum dry to obtain an epoxidation intermediate.

[0041] Step A3: Mix polyetheramine and anhydrous ethanol. During the implementation, polyetheramine D230 is used. The temperature is controlled not higher than 5°C in an ice-water bath. Ultrasonic vibration of 33kHz is applied. The epoxidation intermediate is added to react for 1 hour. The ratio of the epoxidation intermediate, the amino content of the polyetheramine and the anhydrous ethanol is 0.1 mol: 0.23 mol: 70 mL. After the reaction is completed, the ethanol is evaporated under reduced pressure to obtain a modifier.

[0042] Step A4: terephthalic acid, ethylene glycol, modifier and antimony glycol are mixed, nitrogen is introduced for protection, the temperature is raised to 180°C for esterification for 1.5 hours, and then the pressure is reduced to 100 Pa, and the temperature is continued to be raised to 240°C for condensation for 1 hour, wherein the amount ratio of terephthalic acid, ethylene glycol, modifier and antimony glycol is 1 mol: 1.2 mol: 50 g: 0.1 g. After the reaction is completed, the material is discharged, cooled and pelletized under nitrogen protection to obtain modified polyester.

[0043] (2) Preparation of colored yarn

[0044] Step S1: adding the modified polyester into the spinning machine, controlling the temperature of the spinning box to 300±10°C, melt-spinning the modified polyester, cooling it with side-blowing air at a wind temperature of 25°C, cooling and shaping the molten filaments, and winding them to obtain modified filaments.

[0045] Step S2: heat-stretching the modified filaments with two rollers, with the temperature of roller 1 being 95±2°C and the temperature of roller 2 being 125±5°C, controlling the stretching multiple to be 2.5, and cooling and winding to obtain stretched filaments.

[0046] Step S3: The stretched filaments are twice dipped and twice rolled in dye solution for coloring, and then rinsed to remove floating color and then dried to obtain highly sweat-absorbent colored spun yarn.

[0047] Example 3, preparation of high sweat absorption colored spun yarn, the specific implementation process is as follows:

[0048] (1) Preparation of modified polyester

[0049] Step A1: diethanolamine, methyl trifluoroacetate and anhydrous tetrahydrofuran are mixed, dry nitrogen is introduced for protection, the temperature is controlled at 15°C in an ice-water bath, stirring is applied at 150 rpm, equal amounts of sodium hydride are added in three batches, and the addition time is controlled to be 1.6 hours. After complete addition, the temperature is raised to 40±2°C and the reflux reaction is continued for 4.5 hours, wherein the amount ratio of diethanolamine, methyl trifluoroacetate, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.1 mol: 0.4 g: 40 mL. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water, the aqueous phase is removed and vacuum dried to obtain a fluorinated matrix.

[0050] Step A2: Take a fluorinated substrate, epichlorohydrin and dioxane, mix them, pass nitrogen protection, heat to 80°C, apply 90rpm stirring to react for 55 minutes, then cool to 40°C, prepare a saturated aqueous solution of sodium hydroxide, slowly add the aqueous solution of sodium hydroxide, the addition time is 1.2 hours, continue the constant temperature reaction after complete addition, and control the total reaction time of the sodium hydroxide solution to be 3 hours, wherein the amount ratio of the fluorinated substrate, epichlorohydrin, sodium hydroxide and dioxane is 0.1 mol: 0.21 mol: 3.8 g: 70 mL. After the reaction is completed, filter, add water to the filtrate, wash and separate, remove the aqueous phase and vacuum dry to obtain an epoxidation intermediate.

[0051] Step A3: Mix polyetheramine and anhydrous ethanol. During the implementation, polyetheramine D230 is used. The temperature is controlled not higher than 5°C in an ice-water bath. Ultrasonic vibration of 33kHz is applied. The epoxidation intermediate is added to react for 1.1h. The ratio of the epoxidation intermediate, the amino content of the polyetheramine and the anhydrous ethanol is 0.1mol:0.22mol:60mL. After the reaction is completed, the ethanol is evaporated under reduced pressure to obtain a modifier.

[0052] Step A4: Take terephthalic acid, ethylene glycol, modifier and ethylene glycol antimony, mix them, pass nitrogen protection, heat to 175°C for esterification for 1.8 hours, then reduce the pressure to 100 Pa, continue to heat to 230°C, and condense for 1.1 hours, wherein the amount ratio of terephthalic acid, ethylene glycol, modifier and ethylene glycol antimony is 1 mol: 1.28 mol: 44 g: 0.11 g. After the reaction is completed, the material is discharged, cooled and pelletized under nitrogen protection to obtain modified polyester.

[0053] (2) Preparation of colored yarn

[0054] Step S1: adding the modified polyester into the spinning machine, controlling the temperature of the spinning box to 300±10°C, melt-spinning the modified polyester, cooling it with side-blowing air at a wind temperature of 25°C, cooling and shaping the molten filaments, and winding them to obtain modified filaments.

[0055] Step S2: heat-stretching the modified filaments with two rollers, with the temperature of roller 1 being 95±2°C and the temperature of roller 2 being 125±5°C, controlling the stretching multiple to be 2.4, and cooling and winding to obtain stretched filaments.

[0056] Step S3: The stretched filaments are twice dipped and twice rolled in dye solution for coloring, and then rinsed to remove floating color and then dried to obtain highly sweat-absorbent colored spun yarn.

[0057] Comparative Example 1, preparation of colored spun yarn, the specific implementation process is as follows:

[0058] Preparation of polyester: terephthalic acid, ethylene glycol and ethylene glycol antimony are mixed, nitrogen is introduced for protection, the temperature is raised to 190°C for esterification for 2.2 hours, then the pressure is reduced to 100 Pa, the temperature is continued to be raised to 240°C, and polycondensation is carried out for 50 minutes, wherein the amount ratio of terephthalic acid, ethylene glycol and ethylene glycol antimony is 1 mol:1.5 mol:0.12 g. After the reaction is completed, the material is discharged, cooled and pelletized under nitrogen protection to obtain polyester; the specific process for preparing colored yarn is exactly the same as Example 3.

[0059] In comparative example 2, commercially available polyester colored spun yarn was selected, specifically FDY fiber produced by Jiangsu Xinzhanjiang Fiber Technology Co., Ltd.

[0060] Samples were taken from the color-spun fiber material prepared as above, and the mechanical properties were tested using a YG-061-1500 tensile strength tester. The tensile speed was set to 100 mm / min, and the pre-tension was set to 0.05 cN / dtex. The specific test results are shown in Table 1:

[0061] Table 1

[0062]

[0063] It can be seen from the test results in Table 1 that the mechanical strength of the colored spun yarn fiber in the embodiment is slightly lower than that in the comparative example, but still maintains good comprehensive performance and meets the fabric use standards.

[0064] The colored spun yarn prepared above was woven into fabrics according to the warp density of 120 strands / 10cm and the weft density of 160 strands / 10cm. The moisture absorption and quick-drying properties of the fabrics were tested according to GB / T 21655.1-2023 standard. The specific test results are shown in Table 2:

[0065] Table 2

[0066]

[0067] It can be seen from the test results in Table 2 that the colored spun yarn fiber of the embodiment has excellent moisture absorption and quick-drying properties compared with the comparative example.

[0068] Take the above-made fabrics and test the fabric color fastness to soaping and rubbing according to GB / T3921-2008 and GB / T 3920-1997. Use gray card to grade. The specific test results are shown in Table 3:

[0069] Table 3

[0070] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Dry rubbing fastness / grade 5 5 5 3 4 Wet rubbing fastness / grade 4 5 5 3 3 Soap fastness / grade 4 5 4 3 3

[0071] It can be seen from the test results in Table 3 that the colored spun yarn fibers of the embodiments have better color fastness than those of the comparative examples.

[0072] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0073] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A highly sweat-absorbent colored yarn, made by spinning, stretching and dyeing modified polyester, characterized in that: The modified polyester is prepared by the following method: Step A1: diethanolamine, methyl trifluoroacetate and anhydrous tetrahydrofuran are mixed, and dry nitrogen is introduced for protection. The temperature is controlled at 10-20°C in an ice-water bath, and sodium hydride is added in batches with stirring. The addition time is controlled to be 1.2-1.8h. Then, the temperature is raised to 40±2°C and reflux reaction is continued for 4-5h. After the reaction is completed, tetrahydrofuran is removed by rotary evaporation, the substrate is washed with water, the aqueous phase is removed and vacuum dried to obtain a fluorinated substrate; Step A2: Mix the fluorinated substrate, epichlorohydrin and dioxane, introduce nitrogen protection, heat to 75-85°C, stir and react for 40-60 minutes, then cool to 30-40°C, slowly add sodium hydroxide aqueous solution, and control the total reaction time of adding sodium hydroxide aqueous solution to be 2.5-3.5 hours. After the reaction is completed, filter, add water to the filtrate, wash and separate, remove the water phase and vacuum dry to obtain an epoxidation intermediate; Step A3: Mix the polyetheramine and anhydrous ethanol, control the temperature in an ice-water bath to no higher than 5°C, add the epoxidation intermediate under ultrasonic vibration, control the reaction time to be 1-1.3h, and evaporate the ethanol under reduced pressure after the reaction to obtain a modifier; Step A4: terephthalic acid, ethylene glycol, modifier and ethylene glycol antimony are mixed, nitrogen protection is introduced, the temperature is raised to 160-180°C for esterification for 1.5-2h, then the pressure is reduced to 100Pa, the temperature is continued to be raised to 220-240°C, and polycondensation is carried out for 1-1.2h. After the reaction is completed, the material is discharged, cooled and pelletized under nitrogen protection to obtain modified polyester.

2. The high sweat-absorbing colored spun yarn according to claim 1, characterized in that: The usage ratio of diethanolamine, methyl trifluoroacetate, sodium hydride and anhydrous tetrahydrofuran is 0.1 mol: 0.1 mol: 0.36-0.42 g: 35-45 mL.

3. A high sweat-absorbing colored spun yarn according to claim 2, characterized in that: The usage ratio of the fluorinated matrix, epichlorohydrin, sodium hydroxide and dioxane is 0.1 mol: 0.207-0.212 mol: 3.5-4 g: 60-75 mL.

4. The high sweat-absorbing colored spun yarn according to claim 3, characterized in that: The usage ratio of the epoxidation intermediate, the amino content of the polyetheramine and anhydrous ethanol is 0.1 mol: 0.22-0.23 mol: 50-70 mL.

5. The high sweat-absorbing colored spun yarn according to claim 4, characterized in that: The dosage ratio of terephthalic acid, ethylene glycol, modifier and ethylene glycol antimony is 1 mol: 1.2-1.35mol: 40-50g: 0.1-0.12g.

6. A method for preparing a high sweat-absorbing colored spun yarn according to any one of claims 1 to 5, characterized in that: The steps include: Step S1: melt spinning the modified polyester, cooling and shaping it, and winding it to obtain modified filaments; Step S2: thermally stretching the modified filaments with double rollers, cooling and winding the filaments to obtain stretched filaments; Step S3: The stretched filaments are twice dipped and twice rolled in dye solution for coloring, and then rinsed to remove floating color and then dried to obtain highly sweat-absorbent colored spun yarn.

7. The method for preparing a high sweat-absorbing colored spun yarn according to claim 6, characterized in that: During the melt spinning process, the temperature of the spinning box is 300±10℃.

8. The method for preparing a high sweat-absorbing colored spun yarn according to claim 6, characterized in that: The stretching ratio of double-roller heat stretching is 2.2-2.5.