A water-swellable rubber waterstop that is easy to construct and a preparation method thereof

Through the double-layer structure of the water-swellable rubber waterstop, the expansion waterstop layer of polyethylene glycol diacrylate and other materials and the active repair layer of zeolite powder and other materials, combined with a specific protective layer, solve the waterstop problem in the existing technology. The problem of poor effect, affected mechanical properties and lack of self-healing function has achieved efficient and reliable waterproof performance.

CN118581929BActive Publication Date: 2024-10-22HENGSHUI ZHONGTIEJIAN ENG RUBBER
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411067525.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-10-22
Estimated Expiration
2044-08-06

AI Technical Summary

Technical Problem

The existing water-swellable rubber waterstop has limited water-stopping effect when exposed to water, and its mechanical properties are affected. It also lacks self-healing function and is inconvenient to construct. Moreover, repeated expansion and contraction lead to an increase in water seepage channels and reduce the water-stopping performance.

Method used

The water-swellable rubber waterstop adopts a double-layer structure, including an expansion waterstop layer and an active repair layer. The expansion waterstop layer is composed of polyethylene glycol diacrylate, polyether glycol, isocyanate, etc., and the active repair layer is composed of Made of zeolite powder, disodium ethylenediaminetetraacetate and other materials, the protective layer controls degradation through specific materials to ensure long-term waterproofing effect.

Benefits of technology

Optimized water-stopping effect is achieved. The swelling water-stopping layer quickly seals water leakage and forms a solidified layer, which improves mechanical strength and durability. The active repair layer can actively seal the water seepage channel, and the protective layer ensures the proper release of the swelling water-stopping layer, improving the Self-healing ability and long-term waterproof performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118581929B_ABST
    Figure CN118581929B_ABST
Patent Text Reader

Abstract

The present invention discloses a water-swellable rubber waterstop that is easy to construct and a preparation method thereof, comprising a waterstop body, an expansion waterstop layer provided on the waterstop body, an active repair layer provided on the expansion waterstop layer, a protective layer provided on the active repair layer, positioning rings provided at equal intervals on the circumferential side of the waterstop body, and two adjacent waterstop bodies connected by a connecting assembly. The present invention can provide triple protection when in use through the waterstop body, waterproof layer and expansion waterstop layer provided, and has a certain mechanical and mechanical strength through the waterstop body in daily use, and has a water-stopping effect; when water leakage occurs, the expansion waterstop layer expands after contacting with water, and the water leakage is promptly blocked to ensure the water-stopping effect, and the protective layer is provided to effectively prevent the expansion waterstop layer from reacting with water too early, and ensure that the expansion waterstop layer is released at an appropriate time, and a reliable long-term waterproof effect is achieved by accurately controlling the degradation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber waterstops, in particular to a water-swellable rubber waterstop that is easy to construct and a preparation method thereof. Background Art

[0002] During the construction of infrastructure projects, underground facilities and tunnels, due to the shrinkage and expansion of concrete, it is usually necessary to install waterstops in construction joints, settlement joints and deformation joints to prevent water leakage. Existing water-swelling rubber waterstops mainly use bentonite or water-absorbing resin as expansion materials. These materials will swell when exposed to water and fill the gaps to achieve the effect of waterstopping. However, this type of waterstop has the following defects in actual use: First, the waterstop effect is single. Although the waterstop made of bentonite or water-absorbing resin alone can swell when exposed to water, its waterstop effect is limited. When the amount of water seepage is large or the water pressure is high, these materials may not provide enough expansion force to effectively seal the gaps, resulting in poor waterstop effect; secondly, the mechanical and mechanical properties are affected. Although the expansion characteristics of bentonite and water-absorbing resin are helpful for waterstopping, they will have an adverse effect on the overall mechanical and mechanical properties of the rubber waterstop. After expansion, these materials may cause the waterstop to deform, reduce its strength and toughness, and thus affect the long-term stability and durability of the structure. In addition, the existing water-swelling rubber waterstop has problems in the repeated expansion process. It will expand when water enters and shrink when water disappears. This repeated expansion and contraction will form a water seepage channel between the waterstop and the concrete, reducing the water-stopping effect. After repeated expansion and contraction, the water seepage channel will gradually increase, further deteriorating the water-stopping performance. In actual application, the water-swelling waterstop is often constructed in a water state in the early stage. If the material expands in the early stage, it will cause great inconvenience to the construction operation. For example, in Chinese patent CN104177941A, a water-based water-swelling elastic body slow-swelling treatment agent is prepared with styrene-acrylic emulsion as the base resin, which is applied to the surface of the water-swelling elastomer. After the coating film dries, a complete, continuous and dense waterproof isolation layer is formed. The expansion time is controlled by adjusting the thickness of the water-based waterproof isolation layer and the immersion failure time. However, this method requires a complex sand coating process, which is not convenient to construct, and the existing waterstop does not have a self-healing function. When water seeps out of the concrete, it is impossible to actively find the leakage point to close the water seepage channel in the concrete. Summary of the invention

[0003] The object of the present invention is to provide a water-swellable rubber waterstop which is easy to construct and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0004] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a water-swellable rubber waterstop which is easy to construct, comprising a waterstop body, an expansive waterstop layer is provided on the waterstop body, an active repair layer is provided on the expansive waterstop layer, a protective layer is provided on the active repair layer, positioning rings are equidistantly provided on the side surfaces of the waterstop body, and two adjacent waterstop bodies are connected by a connecting assembly.

[0005] Preferably, the connection assembly includes a first connection slope provided at one end of the waterstop body, and a second connection slope provided at the other end of the waterstop body, and two adjacent waterstop bodies are bonded and fixed by the first connection slope and the second connection slope.

[0006] Preferably, the waterstop body is made of one of natural rubber waterstop, EPDM rubber waterstop or PVC waterstop.

[0007] Preferably, the expansion water stop layer is made of the following raw materials in parts by weight:

[0008] 15-25 parts of polyethylene glycol diacrylate, 66-120 parts of polyether diol, 50-55 parts of isocyanate, 15-25 parts of plasticizer, 20-30 parts of acrylamide, 20-30 parts of nano filler and 0.5-2 parts of catalyst.

[0009] Preferably, the polyether diol is selected from a mixture of HSH-204 and HSH-310, with a mass ratio of 1:(1-1.5).

[0010] Preferably, the isocyanate is selected from one of toluene diisocyanate and diphenylmethane diisocyanate; the plasticizer is selected from one of dioctyl phthalate and dibutyl phthalate; the nanofiller is selected from one or more of nano calcium carbonate, kaolin and talc; and the catalyst is one of stannous octoate and dibutyltin dilaurate.

[0011] Preferably, the method for preparing the swelling water-stop layer comprises the following steps:

[0012] S01: Add polyether diol to a three-necked flask, heat to 110-120°C and perform vacuum dehydration for 2-3 hours until there are no rising bubbles in the three-necked flask; then cool to below 60°C, slowly add isocyanate, heat to 80-85°C, reflux at a constant temperature for 2 hours, cool to 40-45°C, discharge and seal to obtain product 1.

[0013] S02: Add polyethylene glycol diacrylate, acrylamide, plasticizer, nano filler and catalyst to the prepolymer, stir evenly, grind on a three-roll grinder, use a scraper fineness meter to detect the fineness to be less than 35 μm, and package to obtain product 2.

[0014] Preferably, the active repair layer is made of the following raw materials in parts by weight:

[0015] 10-20 parts of zeolite powder, 10-20 parts of disodium ethylenediaminetetraacetate, 5-15 parts of sodium citrate, 5-10 parts of magnesium fluorosilicate and 2-6 parts of sodium silicate.

[0016] Preferably, the protective layer comprises the following raw materials in parts by weight:

[0017] 60-96 parts of polyvinyl alcohol, 10-15 parts of polylactic acid, 5-10 parts of silicone crosslinking agent, 5-10 parts of thermoplastic elastomer, and 2-5 parts of tackifying resin.

[0018] Preferably, the organosilicon crosslinking agent is crosslinking agent XR-500, the thermoplastic elastomer includes one of styrene-butadiene-styrene, styrene-isoprene-styrene and POE, and the tackifying resin includes one of C5 petroleum resin, C9 petroleum resin, hydrogenated petroleum resin and terpene resin.

[0019] A method for preparing a water-swellable rubber waterstop that is easy to construct, comprising the following steps:

[0020] S21: Prepare the waterstop body and perform plasma treatment on its surface to improve the activity of the surface.

[0021] S22: Apply product 2 on the main body of the waterstop strip to obtain an expansion waterstop layer with a coating thickness of 0.5-1 cm.

[0022] S23: Mix the components of the active repair layer 3 evenly, and before the product 2 is dry, add 1.3-1.6Kg / m 2 Evenly sprinkle an amount of on the swelling water-stop layer 2 to obtain an active repair layer 3.

[0023] S24: The components of the protective layer 4 are mixed uniformly to obtain a mixture, and then the mixture is put into an extruder for melt extrusion at a temperature of 150-165°C.

[0024] S25: The molten material extruded in S24 is coated on the active repair layer 3 by means of blade coating, with a coating thickness of 0.05-0.2 cm.

[0025] S26: After coating, use heat curing equipment to cure at a temperature of 80-90°C.

[0026] S27: After uniform cooling, rolling and cutting are performed.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1. Double-layer structure achieves optimized water-stopping effect: The present invention includes a waterstop main body and an expansion waterstop layer. In daily use, the waterstop main body provides a basic water-stopping function. When encountering a water leakage, the expansion layer expands rapidly after contacting with water, and can seal the leak in time, thereby effectively ensuring the water-stopping effect and ensuring that the rubber waterstop maintains good mechanical and mechanical strength during use, thereby improving its durability and reliability.

[0029] 2. Emergency response and solidification sealing: The swelling water-stopping layer of the present invention can quickly absorb water and swell when a water leak occurs, effectively blocking the water flow and preventing further water penetration. It not only responds quickly to the water leak, but also forms a solidified layer through hydration reaction, further enhancing the sealing effect and ensuring long-term waterproof performance.

[0030] 3. Active sealing technology: The active layer of the present invention is equipped with materials that can actively identify and seal water seepage channels. It can penetrate into the concrete and react with silicate and aluminate ions to generate insoluble crystalline precipitates, filling microcracks and sealing water seepage channels, greatly improving the self-healing ability and water-stopping efficiency of the waterstop.

[0031] 4. Precisely controlled temporary protective layer: The present invention effectively prevents the swelling water-stop layer from reacting with water too early during the concrete pouring process by setting a protective layer composed of specific materials. The protective layer can be gradually degraded after the concrete solidifies, ensuring that the swelling water-stop layer is released at the appropriate time to achieve the expected sealing effect. Reliable long-term waterproofing effect can be achieved by precisely controlling the degradation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The present invention is a schematic structural diagram of a water-swellable rubber waterstop strip that is easy to construct.

[0033] In the figure: 1. Waterstop body; 2. Swelling waterstop layer; 3. Active repair layer; 4. Protective layer; 5. Positioning ring; 6. Connecting slope one; 7. Connecting slope two. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] See also Figure 1The present invention provides an embodiment: a water-swellable rubber waterstop that is easy to construct and a preparation method thereof, comprising a waterstop body 1, which serves as the base layer of the waterstop, and the material includes a natural rubber waterstop, an EPDM rubber waterstop or a PVC waterstop, which provides basic mechanical strength and preliminary waterproof function, and is a relatively mature technology and will not be described in detail here; an expansion waterstop layer 2 is provided on the waterstop body 1, and an active repair layer 3 is provided on the expansion waterstop layer 2, and a protective layer 4 is provided on the active repair layer 3; positioning rings 5 ​​are equidistantly provided on the sides of the waterstop body 1, which can be conveniently connected with the waterstop body 1. The steel bars are connected and positioned to facilitate the installation of the entire waterstop and avoid deviation. The two adjacent waterstop bodies 1 are connected by a connecting component, which includes a connecting bevel 1 6 opened at one end of the waterstop body 1, and also includes a connecting bevel 2 7 opened at the other end of the waterstop body 1. The two adjacent waterstop bodies 1 are bonded and fixed by connecting bevel 1 6 and connecting bevel 2 7, which can be bonded and fixed by gluing, which facilitates the connection of adjacent waterstop bodies 1, ensures the connection effect while ensuring the sealing, and ensures its waterstop effect.

[0036] According to another aspect of the present invention, the swelling water stop layer 2 is made of the following raw materials in parts by weight:

[0037] 15-25 parts of polyethylene glycol diacrylate, 66-120 parts of polyether diol, 50-55 parts of isocyanate, 15-25 parts of plasticizer, 20-30 parts of acrylamide, 20-30 parts of nano filler and 0.5-2 parts of catalyst.

[0038] Furthermore, the preparation method of the swelling water-stopping layer 2 comprises the following steps:

[0039] S01: Add polyether diol to a three-necked flask and heat it to 110-120°C for vacuum dehydration for 2-3 hours until there are no rising bubbles in the three-necked flask; then cool it to below 60°C, slowly add isocyanate, heat it to 80-85°C, reflux at a constant temperature for 2 hours, cool it to 40-45°C, discharge it, seal it and pack it to obtain product 1.

[0040] S02: Add polyethylene glycol diacrylate, acrylamide, plasticizer, nano filler and catalyst to product one and stir evenly; grind on a three-roll grinder, use a scraper fineness meter to check the fineness to be less than 35 μm and meet the requirements, and package to obtain product two.

[0041] Furthermore, the polyether diol is selected from a mixture of HSH-204 and HSH-310, with a mass ratio of 1:(1-1.5).

[0042] Furthermore, the isocyanate is selected from one of toluene diisocyanate and diphenylmethane diisocyanate.

[0043] The plasticizer is selected from one of dioctyl phthalate and dibutyl phthalate.

[0044] As a preferred embodiment, the amount of plasticizer is 15 to 20 parts by weight.

[0045] The nano filler is selected from one of nano calcium carbonate, kaolin and talc, and is more preferably nano calcium carbonate.

[0046] The catalyst is one of stannous octoate and dibutyltin dilaurate.

[0047] Furthermore, the active repair layer 3 is made of the following raw materials in parts by weight:

[0048] 10-20 parts of zeolite powder, 10-20 parts of disodium ethylenediaminetetraacetate, 5-15 parts of sodium citrate, 5-10 parts of magnesium fluorosilicate and 2-6 parts of sodium silicate.

[0049] Furthermore, the protective layer 4 includes the following raw materials in parts by weight:

[0050] 60-96 parts of polyvinyl alcohol, 10-15 parts of polylactic acid, 5-10 parts of silicone crosslinking agent, 5-10 parts of thermoplastic elastomer and 2-5 parts of tackifying resin.

[0051] Furthermore, the organosilicon cross-linking agent is cross-linking agent XR-500, and the brand is Xirun.

[0052] The thermoplastic elastomer includes one of styrene-butadiene-styrene, styrene-isoprene-styrene, and POE.

[0053] The tackifying resin includes one of C5 petroleum resin, C9 petroleum resin, hydrogenated petroleum resin and terpene resin.

[0054] A method for preparing a water-swellable rubber waterstop that is easy to construct, comprising the following steps:

[0055] S21: Prepare the waterstop body 1 and perform plasma treatment on its surface to improve the surface activity.

[0056] S22: Apply product 2 on the waterstop strip body 1 to obtain an expansion waterstop layer 2 with a coating thickness of 0.5-1 cm.

[0057] S23: Mix the components of the active repair layer 3 evenly, and before the product 2 is dry, add 1.3-1.6Kg / m 2 Evenly sprinkle an amount of on the swelling water-stop layer 2 to obtain an active repair layer 3.

[0058] S24: The components of the protective layer 4 are mixed uniformly to obtain a mixture, and then the mixture is put into an extruder for melt extrusion at a temperature of 150-165°C.

[0059] S25: The molten material extruded in S24 is coated on the active repair layer 3 by means of blade coating, with a coating thickness of 0.05-0.2 cm.

[0060] S26: After coating, use heat curing equipment to cure at a temperature of 80-90°C.

[0061] S27: Cool evenly, then roll up and cut.

[0062] In order to more clearly understand the above technical solution of the present invention, the above solution of the present invention is described in detail below through specific examples.

[0063] Embodiment 1

[0064] According to another aspect of the present invention, a water-swellable rubber waterstop strip that is easy to construct and a preparation method thereof are provided.

[0065] The expansion water-stop layer 2 is made of the following raw materials in parts by weight:

[0066] 15 parts of polyethylene glycol diacrylate, 66 parts of polyether diol, 50 parts of diphenylmethane diisocyanate, 15 parts of plasticizer, 20 parts of acrylamide, 20 parts of nano filler and 0.5 parts of catalyst.

[0067] The mass ratio of polyether diol HSH-204 and HSH-310 is 1:1.

[0068] The preparation method of the expansion water-stop layer 2 comprises the following steps:

[0069] S01: Add polyether diol to a three-necked flask and heat it to 110-120°C for vacuum dehydration for 2-3 hours until there are no rising bubbles in the three-necked flask; then cool it to below 60°C, slowly add isocyanate, heat it to 80-85°C, reflux at a constant temperature for 2 hours, cool it to 40°C, discharge it, seal it and pack it to obtain product 1.

[0070] S02: Add polyethylene glycol diacrylate, acrylamide, plasticizer, nano filler and catalyst to product one and stir evenly; grind on a three-roll grinder, use a scraper fineness meter to check the fineness to be less than 35 μm and meet the requirements, and package to obtain product two.

[0071] The active repair layer 3 is made of the following raw materials in parts by weight:

[0072] 10 parts of zeolite powder, 10 parts of disodium ethylenediaminetetraacetate, 5 parts of sodium citrate, 5 parts of magnesium fluorosilicate and 2 parts of sodium silicate.

[0073] The protective layer 4 comprises the following raw materials in parts by weight:

[0074] 60 parts of polyvinyl alcohol, 10 parts of polylactic acid, 5 parts of silicone crosslinking agent, 5 parts of styrene-butadiene-styrene and 2 parts of tackifying resin.

[0075] A method for preparing a water-swellable rubber waterstop that is easy to construct, comprising the following steps:

[0076] S21: Prepare the waterstop body 1 and perform plasma treatment on its surface to improve the surface activity.

[0077] S22: Apply product 2 on the waterstop strip body 1 to obtain an expansion waterstop layer 2 with a coating thickness of 0.5 cm.

[0078] S23: Mix the components of the active repair layer 3 evenly, and before the product 2 is dry, add 1.3 kg / m 2 Evenly sprinkle an amount of on the swelling water-stop layer 2 to obtain an active repair layer 3.

[0079] S24: The components of the protective layer 4 are mixed uniformly to obtain a mixture, and then the mixture is put into an extruder for melt extrusion at a temperature of 150°C.

[0080] S25: The molten material extruded in S24 is coated on the active repair layer 3 by means of blade coating, with a coating thickness of 0.2 cm.

[0081] S26: After coating, use heat curing equipment to cure at a temperature of 80-90°C.

[0082] S27: Cool evenly, then roll up and cut.

[0083] Embodiment 2

[0084] According to another aspect of the present invention, a water-swellable rubber waterstop strip that is easy to construct and a preparation method thereof are provided.

[0085] The expansion water-stop layer 2 is made of the following raw materials in parts by weight:

[0086] 25 parts of polyethylene glycol diacrylate, 120 parts of polyether diol, 55 parts of toluene diisocyanate, 25 parts of plasticizer, 30 parts of acrylamide, 30 parts of nano filler and 2 parts of catalyst.

[0087] The mass ratio of polyether diol HSH-204 and HSH-310 is 1:1.5.

[0088] The preparation method of the expansion water-stop layer 2 comprises the following steps:

[0089] S01: Add polyether diol to a three-necked flask and heat it to 110-120°C for vacuum dehydration for 2-3 hours until there are no rising bubbles in the three-necked flask. Then cool it to below 60°C, slowly add isocyanate, heat it to 80-85°C, reflux at a constant temperature for 2 hours, cool it to 45°C, and seal and package the product to obtain product 1.

[0090] S02: Add polyethylene glycol diacrylate, acrylamide, plasticizer, nano filler and catalyst to product 1 and mix well. Grind on a three-roll grinder, use a scraper fineness meter to check the fineness to be less than 35 μm, and package to obtain product 2.

[0091] The active repair layer 3 is made of the following raw materials in parts by weight:

[0092] 15 parts of zeolite powder, 15 parts of disodium ethylenediaminetetraacetate, 10 parts of sodium citrate, 7.5 parts of magnesium fluorosilicate and 4 parts of sodium silicate.

[0093] The protective layer 4 comprises the following raw materials in parts by weight:

[0094] 78 parts of polyvinyl alcohol, 12.5 parts of polylactic acid, 7.5 parts of silicone crosslinking agent, 7.5 parts of styrene-isoprene-styrene and 3.5 parts of tackifying resin.

[0095] A method for preparing a water-swellable rubber waterstop that is easy to construct, comprising the following steps:

[0096] S21: Prepare the waterstop body 1 and perform plasma treatment on its surface to improve the surface activity.

[0097] S22: Apply product 2 on the waterstop strip body 1 to obtain an expansion waterstop layer 2 with a coating thickness of 0.8 cm.

[0098] S23: Mix the components of the active repair layer 3 evenly, and before the product 2 is dry, add 1.6Kg / m 2 Evenly sprinkle an amount of on the swelling water-stop layer 2 to obtain an active repair layer 3.

[0099] S24: The components of the protective layer 4 are mixed uniformly to obtain a mixture, and then the mixture is put into an extruder for melt extrusion at an extrusion temperature of 165°C.

[0100] S25: The molten material extruded in S24 is coated on the active repair layer 3 by means of blade coating, with a coating thickness of 0.1 cm.

[0101] S26: After coating, use heat curing equipment to cure at a temperature of 80-90°C.

[0102] S27: Cool evenly, then roll up and cut.

[0103] Embodiment 3

[0104] According to another aspect of the present invention, a water-swellable rubber waterstop strip that is easy to construct and a preparation method thereof are provided.

[0105] The expansion water-stop layer 2 is made of the following raw materials in parts by weight:

[0106] 18 parts of polyethylene glycol diacrylate, 100 parts of polyether diol, 51 parts of toluene diisocyanate, 25 parts of plasticizer, 30 parts of acrylamide, 30 parts of nano filler and 2 parts of catalyst.

[0107] The mass ratio of polyether diol HSH-204 and HSH-310 is 1:1.4.

[0108] The preparation method of the expansion water-stop layer 2 comprises the following steps:

[0109] S01: Add polyether diol to a three-necked flask and heat it to 110-120°C for vacuum dehydration for 2-3 hours until there are no rising bubbles in the three-necked flask; then cool it to below 60°C, slowly add isocyanate, heat it to 80-85°C, reflux at a constant temperature for 2 hours, cool it to 42°C, and seal and package the discharged material to obtain product 1.

[0110] S02: Add polyethylene glycol diacrylate, acrylamide, plasticizer, nano filler and catalyst to product one and stir evenly; grind on a three-roll grinder, use a scraper fineness meter to check the fineness to be less than 35 μm and meet the requirements, and package to obtain product two.

[0111] Furthermore, the active repair layer 3 is made of the following raw materials in parts by weight:

[0112] 20 parts of zeolite powder, 20 parts of disodium ethylenediaminetetraacetate, 15 parts of sodium citrate, 10 parts of magnesium fluorosilicate and 6 parts of sodium silicate.

[0113] Furthermore, the protective layer 4 includes the following raw materials in parts by weight:

[0114] 96 parts of polyvinyl alcohol, 15 parts of polylactic acid, 10 parts of silicone crosslinking agent, 10 parts of POE, and 5 parts of tackifying resin.

[0115] A method for preparing a water-swellable rubber waterstop that is easy to construct, comprising the following steps:

[0116] S21: Prepare the waterstop body 1 and perform plasma treatment on its surface to improve the surface activity.

[0117] S22: Apply product 2 on the waterstop strip body 1 to obtain an expansion waterstop layer 2 with a coating thickness of 1 cm.

[0118] S23: Mix the components of the active repair layer 3 evenly, and before the product 2 is dry, add 1.5 kg / m 2 Evenly sprinkle an amount of on the swelling water-stop layer 2 to obtain an active repair layer 3.

[0119] S24: The components of the protective layer 4 are mixed uniformly to obtain a mixture, and then the mixture is put into an extruder for melt extrusion at an extrusion temperature of 160°C.

[0120] S25: The molten material extruded in S24 is coated on the active repair layer 3 by means of blade coating, with a coating thickness of 0.05 cm.

[0121] S26: After coating, use heat curing equipment to cure at a temperature of 80-90°C.

[0122] S27: After curing, the film and substrate are cooled evenly to avoid the generation of internal stress, and then rolled and cut.

[0123] Embodiment 4

[0124] The difference from the first embodiment is that the expansion water stop layer 2 is made of the following raw materials in parts by weight:

[0125] 20 parts of polyethylene glycol diacrylate, 90 parts of polyether diol, 54 parts of diphenylmethane diisocyanate, 24 parts of plasticizer, 24 parts of acrylamide, 24 parts of nano filler and 1.4 parts of catalyst.

[0126] The mass ratio of polyether diol HSH-204 and HSH-310 is 1:1.3.

[0127] Embodiment 5

[0128] The difference from the first embodiment is that the expansion water stop layer 2 is made of the following raw materials in parts by weight:

[0129] 22 parts of polyethylene glycol diacrylate, 80 parts of polyether diol, 53 parts of diphenylmethane diisocyanate, 24 parts of plasticizer, 26 parts of acrylamide, 26 parts of nano filler and 1.3 parts of catalyst.

[0130] The mass ratio of polyether diol HSH-204 and HSH-310 is 1:1.2.

[0131] Comparative Example 1

[0132] The protective layer 4 is not provided, and the rest is the same as that of the first embodiment.

[0133] Comparative Example 2

[0134] The protective layer 4 and the active repair layer 3 are not provided, and the rest are the same as those in the first embodiment.

[0135] Comparative Example 3

[0136] The expansion water stop layer 2 is composed of the following components:

[0137] 100 parts of natural rubber, 30 parts of white carbon black, 15 parts of plasticizer, 15 parts of acrylamide, 0.8 parts of S, 0.8 parts of CZ, and 0.6 parts of DM; the rest are the same as in Example 1.

[0138] Comparative Example 4

[0139] The swelling water-stop layer 2 is made of the following raw materials in parts by weight: 110 parts of polyether diol, 20 parts of isocyanate, 15 parts of plasticizer, 15 parts of acrylamide, 5 parts of nano filler and 0.04 parts of catalyst; the rest are the same as those in Example 1.

[0140] Comparative Example 5

[0141] The active repair layer 3 is made of the following raw materials in parts by weight: 20 parts of disodium ethylenediaminetetraacetate, 5 parts of sodium citrate, 5 parts of magnesium fluorosilicate and 2 parts of sodium silicate; the rest is the same as that in the first embodiment.

[0142] Comparative Example 6

[0143] The active repair layer 3 is made of the following raw materials in parts by weight: 5 parts of zeolite powder, 25 parts of disodium ethylenediaminetetraacetate, 2 parts of sodium citrate, 10 parts of magnesium fluorosilicate and 6 parts of sodium silicate; the rest are the same as those in Example 1.

[0144] Comparative Example 7

[0145] The protective layer 4 is made of the following raw materials in parts by weight: 60 parts of polyvinyl alcohol, 10 parts of polylactic acid, 5 parts of organic silicon cross-linking agent and 2 parts of tackifying resin; the rest are the same as those in the first embodiment.

[0146] The volume expansion ratio of the swelling water-stop layer 2 is tested in accordance with Appendix A of GB / T18173.3-2014, and samples with different immersion times (immersion for 24h, 72h, and 28d) are tested respectively; the volume expansion ratio after repeated immersion test is tested according to the following steps: the sample is immersed in distilled water at room temperature (23±5)℃ for 16h, taken out and dried at (70±2)℃ for 8h, then immersed in water for 16h, and then dried for 8h; the sample is immersed in water repeatedly, and the volume expansion ratio is measured after 4 cycles.

[0147] Anti-seepage performance: The protective layer of the present invention is used as the water-facing surface and pre-buried into 1 / 2 of the height of the anti-seepage test piece, and then a curing test is carried out according to the experimental method of GB / T 50082-2009.

[0148]

[0149] Through the above experiments, it can be known that when the protective layer 4 is not added, when the rubber waterstop is installed and poured with concrete, the swelling waterstop layer 2 will react with the water in the concrete prematurely, which will affect the expansion ratio during subsequent water leakage, and thus affect the water-stopping effect; when the raw material components and proportions of the protective layer 4 are changed, the temporary protection effect of the protective layer 4 decreases; when the protective layer active repair layer 3 is not set, the anti-permeability performance will decrease, and the swelling waterstop layer 2 will be replaced by ordinary rubber-based swelling rubber. The initial expansion multiple increases rapidly. After repeated immersion tests, the volume expansion ratio decreases significantly compared to the 28d data. On the one hand, it shows that ordinary rubber-based swelling rubber will affect the construction quality, have poor durability, and reduce the anti-permeability performance; under the raw materials and proportions of the active layer of the present invention, the anti-permeability performance will be better, and the anti-permeability performance will decrease if the raw materials and proportions are changed.

[0150] In summary, the double-layer structure of the present invention achieves an optimized water-stopping effect: the present invention includes a water-stop strip body 1, which provides a basic water-stopping function in daily use. When a water leakage occurs, the swelling water-stop layer 2 rapidly expands after contacting with water, and can timely block the water leakage, thereby effectively ensuring the water-stopping effect and improving its durability and reliability; the swelling water-stop layer 2 can quickly absorb moisture and expand when a water leakage occurs, effectively blocking the water flow and preventing further penetration of moisture, which not only responds quickly to the water leakage, but also forms a solidified layer through a hydration reaction, further enhancing the sealing effect and ensuring long-term waterproofing. Performance: The active layer is equipped with materials that can actively identify and close water seepage channels, penetrate into the concrete, and react with silicate and aluminate ions to generate insoluble crystalline precipitates. This precipitate can effectively fill microcracks and close water seepage channels, greatly improving the self-healing ability and water-stopping efficiency of the waterstop. The protective layer 4 effectively prevents the swelling waterstop layer 2 from reacting with water too early during the concrete pouring process. The protective layer 4 can gradually degrade after the concrete solidifies, ensuring that the swelling waterstop layer 2 is released at the appropriate time to achieve the expected sealing effect, and achieve reliable long-term waterproofing effect by precisely controlling the degradation process.

[0151] It is obvious to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be regarded as exemplary and non-restrictive from any point of view, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention, and any reference numerals in the claims should not be regarded as limiting the claims involved.

Claims

1. A water-swellable rubber waterstop that is easy to construct, comprising a waterstop body (1), Features: The waterstop strip body (1) is provided with an expansion waterstop layer (2), an active repair layer (3) is provided on the expansion waterstop layer (2), a protective layer (4) is provided on the active repair layer (3), positioning rings (5) are equidistantly provided on the circumferential side of the waterstop strip body (1), and two adjacent waterstop strip bodies (1) are connected via a connecting assembly; the expansion waterstop layer (2) is made of the following raw materials in parts by weight: 15-25 parts of polyethylene glycol diacrylate, 66-120 parts of polyether diol, 50-55 parts of isocyanate, and 15-25 parts of plasticizer. parts, acrylamide 20-30 parts, nano filler 20-30 parts and catalyst 0.5-2 parts; the active repair layer (3) is made of the following raw materials in parts by weight: zeolite powder 10-20 parts, disodium ethylenediaminetetraacetate 10-20 parts, sodium citrate 5-15 parts, magnesium fluorosilicate 5-10 parts and sodium silicate 2-6 parts; the protective layer (4) comprises the following raw materials in parts by weight: polyvinyl alcohol 60-96 parts, polylactic acid 10-15 parts, silicone crosslinking agent 5-10 parts, thermoplastic elastomer 5-10 parts and tackifying resin 2-5 parts.

2. A water-swellable rubber waterstop that is easy to construct according to claim 1, Features: The connection assembly comprises a connection bevel 1 (6) provided at one end of the waterstop strip body (1), and also comprises a connection bevel 2 (7) provided at the other end of the waterstop strip body (1), and two adjacent waterstop strip bodies (1) are bonded and fixed by means of the connection bevel 1 (6) and the connection bevel 2 (7).

3. The water-swellable rubber waterstop strip that is easy to construct according to claim 1, Features: The waterstop main body (1) is made of one of a natural rubber waterstop, an EPDM rubber waterstop or a PVC waterstop.

4. The water-swellable rubber waterstop strip that is easy to construct according to claim 1, Features: The isocyanate is selected from one of toluene diisocyanate and diphenylmethane diisocyanate; the plasticizer is selected from one of dioctyl phthalate and dibutyl phthalate; the nano filler is selected from one of nano calcium carbonate, kaolin and talc; and the catalyst is one of stannous octoate and dibutyltin dilaurate.

5. The water-swellable rubber waterstop strip that is easy to construct according to claim 1, Features: The method for preparing the swelling water-stopping layer (2) comprises the following steps: S01: Add polyether diol to a three-necked flask and heat it to 110-120°C for vacuum dehydration for 2-3 hours until there are no rising bubbles in the three-necked flask; then cool it to below 60°C, slowly add isocyanate, heat it to 80-85°C, reflux at a constant temperature for 2 hours, cool it to 40-45°C, and seal and package the discharged material to obtain product 1; S02: Add polyethylene glycol diacrylate, acrylamide, plasticizer, nano filler and catalyst to product one and stir evenly; grind on a three-roll grinder, use a scraper fineness meter to check the fineness to be less than 35 μm and meet the requirements, and package to obtain product two.

6. The water-swellable rubber waterstop strip that is easy to construct according to claim 1, Features: The organosilicon crosslinking agent is crosslinking agent XR-500, the thermoplastic elastomer includes one of styrene-butadiene-styrene, styrene-isoprene-styrene and POE, and the tackifying resin includes one of C5 petroleum resin, C9 petroleum resin, hydrogenated petroleum resin and terpene resin.

7. A method for preparing a water-swellable rubber waterstop that is easy to construct as described in any one of claims 5-6, It is characterized in that The following steps are involved: S21: preparing a water stop strip body (1), and performing plasma treatment on the surface thereof to improve the activity of the surface; S22: coating the second product on the waterstop strip body (1) to obtain an expansion waterstop layer (2) with a coating thickness of 0.5-1 cm; S23: Mix the components of the active repair layer (3) evenly, and before the product is dry, add 1.3-1.6 kg / m 2 Evenly sprinkle the amount of the active repair layer (3) on the swelling water stop layer (2); S24: mixing the components of the protective layer (4) uniformly to obtain a mixture, and then placing the mixture into an extruder for melt extrusion at a temperature of 150-165° C.; S25: coating the molten material extruded from S24 on the active repair layer (3) by means of blade coating, with a coating thickness of 0.05-0.2 cm; S26: After coating, use heat curing equipment to cure at a temperature of 80-90°C; S27: Cool evenly, then roll up and cut.

Citation Information

Patent Citations

  • Water-based water swelling elastomer swell-slowing treating agent and preparation method thereof

    CN104177941A

  • Composite rubber waterstop

    CN112727506A

  • Replacing structure for rubber waterstop of pool expansion joint

    CN219569212U

  • Combined waterstop

    CN221168190U

  • Rubber waterproof belt with expansion when in water

    CN2238868Y