All-solid-state battery positive electrode sheet and preparation method thereof, and all-solid-state battery
By adopting the multi-layered adhesive distribution in the positive electrode sheet of the all-solid state battery, the problem of inconsistent interface durability of the positive electrode active material and the electrolyte is solved, and the high energy density and long cycle life of the all-solid state battery are achieved.
Patent Information
- Application Number
- CN202411052757.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The all-solid-state battery positive plate cannot ensure that the interface durability of the positive electrode active material and electrolyte is the same throughout the thickness during the battery cycle, resulting in performance deterioration and safety problems.
The positive electrode material layer adopts a multi-layer structure, including the adhesive distribution of two sub-layers. By controlling the molecular weight, viscosity and drying temperature of the adhesive, ensure that the adhesive is linearly distributed along the longitudinal direction, and the interface gradient distribution is achieved, thereby Improve interface durability and cycle stability.
It effectively improves the interface durability and circulation performance of the positive electrode sheet of all solid state battery, ensuring the high energy density and long cycle life of the battery.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of all-solid-state batteries, and in particular to an all-solid-state battery positive electrode sheet and a preparation method thereof, and an all-solid-state battery. Background Art
[0002] All-solid-state batteries, that is, batteries in which the electrodes and electrolytes are solid within the operating temperature range and do not contain any liquid components, have higher energy density and better long-term cycle performance.
[0003] The positive electrode of an all-solid-state battery is usually composed of a positive electrode active material and a solid electrolyte. During the charge and discharge cycles of the all-solid-state battery, the positive electrode active material particles undergo repeated volume expansion or contraction, which makes the interface between the positive electrode active material and the solid electrolyte unstable. The common layered positive electrode oxide material is highly deformed (up to 8%) due to lithium deintercalation, which easily causes the interface between the positive electrode active material and the solid electrolyte to debond. Interface debonding is the main cause of performance degradation and safety issues in all-solid-state batteries, and this interface debonding phenomenon is particularly evident in high-load positive electrode designs.
[0004] In response to the above problems, existing studies have proposed electrolyte modification, including adding lithium salt additives and other additives; constructing multilayer polymer electrolytes; multilayer positive electrode design, etc., to construct a stable positive electrode-electrolyte intermediate phase. However, these methods are complex, and multilayer design is prone to interface problems between layers, and gradient design cannot be fully achieved. The binder content between layers often has a jump-like growth, and it is impossible to ensure that the interface durability between the positive electrode active material and the electrolyte is the same throughout the thickness. Summary of the invention
[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides an all-solid-state battery positive electrode sheet and a preparation method thereof, and an all-solid-state battery, so as to solve the problems that the existing all-solid-state battery positive electrode sheet cannot ensure that the interface durability between the positive electrode active material and the electrolyte is the same throughout the thickness during the battery cycle, resulting in degradation of the performance of the all-solid-state battery.
[0006] To achieve the above and related purposes, the present invention adopts the following technical solutions:
[0007] The first aspect of the present invention provides an all-solid-state battery positive electrode sheet, comprising a positive electrode current collector and a positive electrode material layer formed on the surface of the positive electrode current collector, wherein the positive electrode material layer comprises a binder; the positive electrode material layer comprises a positive electrode first sublayer and a positive electrode second sublayer, wherein the positive electrode first sublayer is located between the positive electrode current collector and the positive electrode second sublayer;
[0008] When the thickness of the positive electrode sheet is H μm, the thickness of the first positive electrode sublayer and the second positive electrode sublayer is 0.2H μm, and the binder content of the first positive electrode sublayer is X awt%, the binder content of the second sublayer of the positive electrode is X b wt%, the positive electrode satisfies the following relationship I:
[0009] -0.05≤X a +0.23- X b ≤0.05.
[0010] Further, the range of H is 50 μm ≤ H ≤ 300 μm.
[0011] Furthermore, the peeling force of the first sublayer of the positive electrode is Y a N / m, the peeling force of the second sublayer of the positive electrode is Y b N / m, the positive electrode satisfies the following relationship II:
[0012] -1≤Y a +1.5- Y b ≤1.
[0013] Furthermore, the positive electrode first sublayer and the positive electrode second sublayer are adjacent sublayers.
[0014] Furthermore, the binder content of the positive electrode material layer satisfies at least one of the following conditions (a) to (b):
[0015] (a) The mass ratio of the binder to the positive electrode material layer is (3-5):100;
[0016] (b) The content of the binder increases from close to the positive electrode current collector to away from the positive electrode current collector.
[0017] Furthermore, the positive electrode material layer also includes a solid electrolyte, a positive electrode active material and a conductive agent, wherein:
[0018] The solid electrolyte is selected from at least one of an oxide solid electrolyte, a sulfide solid electrolyte and a halide solid electrolyte;
[0019] The positive electrode active material is selected from at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and lithium-rich manganese-based oxide;
[0020] The conductive agent is selected from at least one of graphite, graphene, carbon black, carbon fiber and carbon nanotube;
[0021] The binder is selected from at least one of styrene-butadiene rubber, sodium alginate, polyacrylonitrile, polyurethane, polyacrylic acid, ethylene-propylene-diene monomer, styrene-butadiene rubber, polyvinyl methacrylate glycerol methacrylate copolymer, hydrogenated nitrile rubber, nitrile rubber, poly(acrylic acid-poly(ethylene glycol) methyl ether methacrylate) copolymer, polyvinylidene fluoride and polyvinylidene fluoride copolymer.
[0022] A second aspect of the present invention provides a method for preparing a positive electrode sheet of an all-solid-state battery, comprising the following steps:
[0023] (1) Preparing positive electrode slurry: dissolving the binder in an organic solvent to obtain a binder paste;
[0024] The binder glue and the positive electrode material composition are mixed to obtain a positive electrode slurry, wherein:
[0025] The molecular weight of the binder is 500000 Da~1200000 Da, and the viscosity of the binder is 3000 mPa·S~3500 mPa·S;
[0026] The vapor pressure of organic solvents is 1.5 kPa~3 kPa;
[0027] (2) coating the positive electrode slurry on the surface of the positive electrode current collector, drying, and preparing a positive electrode material layer to obtain a positive electrode sheet for an all-solid-state battery, wherein:
[0028] The drying temperature is 120℃~150℃;
[0029] The mass ratio of the binder to the positive electrode material layer is (3~5):100.
[0030] According to the above technical means, when the molecular weight of the binder of the present application is within the above range, the binder has high bonding strength and durability, and can effectively control the sedimentation rate of each component in the positive electrode slurry, thereby adjusting the binder content along the direction from close to the positive electrode collector to away from the positive electrode collector, that is, longitudinally, and increasing distribution; at the same time, the binder that meets the above conditions can improve the interface contact of each component of the positive electrode sheet of the all-solid-state battery, and improve the cycle stability and fast charging performance of the all-solid-state battery. When the viscosity of the binder is within the above range, it can also effectively adjust the sedimentation rate of each component in the positive electrode slurry, thereby achieving the adjustment of the content distribution of the binder in the positive electrode material layer. At the same time, the present application controls the molecular weight and viscosity of the binder and the vapor pressure of the organic solvent to meet the above range, which is conducive to the increasing distribution of the binder content along the direction from close to the positive electrode collector to away from the positive electrode collector; secondly, the simultaneous satisfaction of the above conditions can make the local distribution of the binder inside the positive electrode material layer relatively consistent, and avoid the sudden change of the binder component in the positive electrode material layer due to the adjustment of the process parameters, thereby affecting the cycle stability of the battery.
[0031] In addition, the present application controls the drying temperature to meet the above range to effectively improve the performance of the battery. If the drying temperature is lower than the above range, the binder cannot be distributed linearly in the longitudinal direction, and the interface durability of the components inside the positive electrode sheet of the all-solid-state battery is different throughout the thickness, causing the components inside the positive electrode sheet of the all-solid-state battery near the negative electrode side to be prone to interface debonding. If the drying temperature is higher than the above range, the binder will float up very quickly, causing the binder content near the positive electrode collector side to be too low, thereby making the adhesion between the collector and the positive electrode active material poor, and then causing the positive electrode film of the all-solid-state battery to fall off, and the all-solid-state battery cannot be prepared.
[0032] Moreover, when the mass ratio of the binder to the positive electrode material layer of the present application meets the above ratio, it can maintain good adhesion between the positive electrode material layer and the positive electrode collector without increasing the resistance of the positive electrode sheet of the all-solid-state battery.
[0033] Furthermore, in step (1), the polarity parameter of the organic solvent is 0-4.5.
[0034] According to the above technical means, the present application controls the polarity of the organic solvent within the above range to avoid the problem of solid electrolyte decomposition caused by excessive polarity of the organic solvent and to improve the ion transfer efficiency inside the positive electrode of the all-solid-state battery.
[0035] Furthermore, in step (1), the positive electrode material composition includes a positive electrode active material, a solid electrolyte and a conductive agent.
[0036] A third aspect of the present invention provides an all-solid-state battery, comprising the all-solid-state battery positive electrode sheet as described above, or, comprising the all-solid-state battery positive electrode sheet prepared according to the above preparation method.
[0037] The beneficial technical effects of the present invention are:
[0038] The present invention allows the binder to be linearly distributed in the longitudinal direction of the positive electrode material layer by optimizing the binder, organic solvent and drying temperature, thereby forming an all-solid-state battery positive electrode sheet with a gradient distribution of the binder content in situ, and further making the peeling force between the sublayers in the positive electrode material layer also present a linear distribution trend, so as to ensure that the interface durability of each component inside the positive electrode sheet of the all-solid-state battery is the same throughout the thickness, improve the consistency of the positive electrode, and further improve the capacity and cycle performance of the all-solid-state battery.
[0039] The preparation method of the present invention has a simple process and can form an all-solid-state battery positive electrode sheet with a gradient distribution of binder content in situ in only one step. The good interface contact of the components inside the all-solid-state battery positive electrode sheet can be maintained during the battery cycle, thereby developing a high-energy density all-solid-state battery with a long cycle life and high-rate performance.
[0040] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. DETAILED DESCRIPTION
[0041] Unless otherwise defined, all technical and / or scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the invention belongs. It should be understood that certain features of the invention (described in the context of separate embodiments for clarity) may also be provided in combination in a single embodiment. On the contrary, multiple features of the invention (described in the context of a single embodiment for brevity) may also be provided separately or in any suitable combination or in any other described embodiment of the invention when appropriate. Certain features described in the context of various embodiments will not be considered as essential features of those embodiments unless the embodiment is inoperable without those elements. The present invention is further described below by specific specific examples, but it should be noted that the specific process conditions and results described in the embodiments of the present invention are only used to illustrate the present invention, and cannot be used to limit the scope of protection of the present invention. All equivalent changes or modifications made according to the spirit and essence of the present invention should be included in the scope of protection of the present invention.
[0042] First of all, it should be noted that the materials used in the examples and comparative examples of the present application are all commercially available.
[0043] The polarity parameters of the organic solvents in this application are based on the following common solvent polarity table 1:
[0044] Table 1 Polarity of common solvents
[0045]
[0046] The present invention provides a method for preparing an all-solid-state battery positive electrode sheet, comprising the following steps:
[0047] (1) Prepare positive electrode slurry: dissolve the binder in an organic solvent to obtain a binder paste with a concentration of 1% to 30%;
[0048] Mixing the binder glue, the cathode material composition and the solvent in a glove box using a high-speed stirrer to obtain a cathode slurry;
[0049] (2) Use a scraper to coat the positive electrode slurry on the positive electrode current collector, quickly transfer it to a vacuum state, dry it, and prepare a positive electrode material layer to obtain an all-solid-state battery positive electrode sheet.
[0050] In one embodiment of the present application, in step (1), the molecular weight of the binder is 500000 Da~1200000 Da, for example, it can be 500000 Da, 600000 Da, 700000 Da, 800000 Da, 900000 Da, 1000000 Da, 1100000 Da, 1200000 Da, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0051] The viscosity of the adhesive is 3000 mPa·S ~ 3500 mPa·S. For example, it can be 3000 mPa·S, 3100 mPa·S, 3200 mPa·S, 3300 mPa·S, 3400 mPa·S, 3500 mPa·S, but is not limited to the listed values, and other values not listed within the above range are also applicable.
[0052] The present application limits the molecular weight of the binder to effectively reduce the amount of binder used without reducing adhesion. In addition, the present application limits the viscosity of the binder because a binder with low viscosity will cause the internal resistance of the battery to decrease, increase the fluidity of the electrode material, and thus reduce the reliability and safety of the battery. A binder with high viscosity will increase the internal resistance of the battery, reduce the electrochemical performance of the battery, and extend the charging time of the battery. Therefore, the present application limits the viscosity of the binder to meet the above range, which will not affect the internal resistance and electrochemical performance of the battery while facilitating homogenization and maintaining the stability of the slurry.
[0053] In one embodiment of the present application, in step (1), the binder is selected from at least one of styrene-butadiene rubber, sodium alginate, polyacrylonitrile, polyurethane, polyacrylic acid, ethylene-propylene-diene monomer, styrene-butadiene rubber, polyvinyl methacrylate glycerol isomethacrylate copolymer, hydrogenated nitrile rubber, nitrile rubber, poly(acrylic acid-poly(ethylene glycol) methyl ether methacrylate) copolymer, polyvinylidene fluoride and polyvinylidene fluoride copolymer.
[0054] In one embodiment of the present application, in step (1), the vapor pressure of the organic solvent is 1.5 kPa to 3 kPa. For example, it can be 1.5 kPa, 1.6 kPa, 1.9 kPa, 2 kPa, 2.2 kPa, 2.5 kPa, 2.8 kPa, 3 kPa, but is not limited to the listed values, and other values not listed in the above numerical range are also applicable.
[0055] The application limits the vapor pressure of the organic solvent, which is conducive to promoting the linear distribution of the binder in the longitudinal direction. If the vapor pressure is too low, the volatilization rate of the organic solvent is too slow, resulting in uneven distribution of the binder; if the vapor pressure is too high, the binder will accumulate on the surface of the positive electrode of the all-solid-state battery, increase the interface resistance between the positive electrode of the all-solid-state battery and the solid electrolyte, and easily cause the positive electrode material layer to debond from the positive electrode current collector.
[0056] In one embodiment of the present application, in step (1), the polarity parameter of the organic solvent is 0-4.5. For example, it can be 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4, 4.5, but is not limited to the listed values, and other values not listed in the above numerical range are also applicable.
[0057] The present application controls the polarity of the organic solvent to avoid the problem of solid electrolyte decomposition caused by excessive polarity of the organic solvent, and improves the ion transmission efficiency inside the positive electrode of the all-solid-state battery.
[0058] In one embodiment of the present application, in step (1), the speed of the high-speed stirrer is 500 rpm~2000 rpm, and the mixing time is 1 min~30 min.
[0059] In one embodiment of the present application, in step (1), the solid content of the positive electrode slurry is 30% to 80%. For example, it can be 30%, 40%, 50%, 60%, 70%, 80%, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0060] In one embodiment of the present application, in step (1), the positive electrode material composition includes a positive electrode active material, a solid electrolyte and a conductive agent, wherein:
[0061] The positive electrode active material is selected from one or more of binary metal oxides, ternary metal oxides and quaternary metal oxides.
[0062] Further preferably, the positive electrode active material is selected from one or more of lithium cobalt oxide (LCO), lithium nickel oxide (LNO), lithium manganese oxide (LMO), lithium nickel manganese oxide (LNMO), lithium nickel cobalt manganese oxide (NCM), lithium nickel cobalt aluminum oxide (NCA) and lithium rich manganese-based oxide (LRMO).
[0063] The solid electrolyte is selected from one or more of an oxide solid electrolyte, a sulfide solid electrolyte and a halide solid electrolyte.
[0064] The conductive agent is selected from one or more of graphite, graphene, carbon black, carbon fiber and carbon nanotube.
[0065] Preferably, the conductive agent includes carbon black and carbon fiber, and the mass ratio of carbon black to carbon fiber is 1:(0.2-1.5), preferably 1:1.
[0066] Further preferably, the carbon black is conductive carbon black (SP, super p); the carbon fiber is at least one of carbon nanofiber (CNF), vapor grown carbon fiber (VGCF), and vapor grown carbon nanofiber (VGCNF).
[0067] In one embodiment of the present application, the mass ratio of the positive electrode active material, the solid electrolyte, the conductive agent and the binder is (60-90): (5-30): (1-5): (3-5).
[0068] In one embodiment of the present application, in step (2), the mass ratio of the binder to the positive electrode material layer is (3-5): 100. The present application controls the binder content to maintain good adhesion between the positive electrode material layer and the positive electrode current collector while not increasing the resistance of the positive electrode sheet of the all-solid-state battery.
[0069] In one embodiment of the present application, in step (2), the positive electrode current collector is a carbon-coated aluminum foil.
[0070] In one embodiment of the present application, in step (2), the drying temperature is 120°C~150°C, for example, it can be 120°C, 130°C, 140°C, 150°C, but is not limited to the listed values. Other values not listed within the above numerical range are also applicable.
[0071] The present application controls the drying temperature to effectively improve the performance of the battery. If the drying temperature is lower than the above range, the binder cannot be distributed linearly in the longitudinal direction, and the interface durability of each component inside the positive electrode sheet of the all-solid-state battery is different throughout the thickness, causing the components inside the positive electrode sheet of the all-solid-state battery near the negative electrode side to easily debond at the interface. If the drying temperature is higher than the above range, the binder will float up very quickly, causing the binder content near the positive electrode collector side to be too low, resulting in poor adhesion between the collector and the positive electrode active material, and then causing the positive electrode film of the all-solid-state battery to fall off, and the all-solid-state battery cannot be prepared.
[0072] In one embodiment of the present application, the drying time is 12 h to 24 h.
[0073] In one embodiment of the present application, the surface capacity of the positive electrode sheet of the all-solid-state battery prepared in the present application is 1-10 mAh / cm 2 .
[0074] The present invention also provides an all-solid-state battery positive electrode sheet, which is prepared according to the above preparation method. The all-solid-state battery positive electrode sheet of the present invention comprises a positive electrode current collector and a positive electrode material layer formed on the surface of the positive electrode current collector, the positive electrode material layer comprises a binder; the positive electrode material layer comprises a positive electrode first sublayer and a positive electrode second sublayer, the positive electrode first sublayer is located between the positive electrode current collector and the positive electrode second sublayer;
[0075] When the thickness of the positive electrode sheet is H μm, the thickness of the first positive electrode sublayer and the second positive electrode sublayer is 0.2H μm, and the binder content of the first positive electrode sublayer is X a wt%, the binder content of the second sublayer of the positive electrode is X b wt%, the positive electrode satisfies the following relationship I:
[0076] -0.05≤X a +0.23- X b ≤0.05.
[0077] In one embodiment of the present application, the range of H is 50 μm ≤ H ≤ 300 μm.
[0078] In one embodiment of the present application, the peeling force of the first sub-layer of the positive electrode is Y a N / m, the peeling force of the second sublayer of the positive electrode is Y b N / m, the positive electrode satisfies the following relationship II:
[0079] -1≤Y a +1.5- Y b ≤1.
[0080] In one embodiment of the present application, the positive electrode first sublayer and the positive electrode second sublayer are adjacent sublayers.
[0081] In one embodiment of the present application, the binder content of the positive electrode material layer satisfies at least one of the following conditions (a) to (b):
[0082] (a) The mass ratio of the binder to the positive electrode material layer is (3-5):100;
[0083] (b) The content of the binder increases from close to the positive electrode current collector to away from the positive electrode current collector.
[0084] It should be noted that the sub-layers of the all-solid-state battery positive electrode sheet of the present invention are based on artificial divisions rather than physical stratification. Therefore, as an example, the all-solid-state battery positive electrode sheet of the present invention may include a first positive electrode sub-layer, a second positive electrode sub-layer, a third positive electrode sub-layer, a fourth positive electrode sub-layer, and a fifth positive electrode sub-layer.
[0085] In one embodiment of the present application, the positive electrode sheet of the all-solid-state battery of the present invention is preferably a thick electrode sheet. On this basis, the positive electrode sheet satisfies the above-mentioned equations Ⅰ and Ⅱ.
[0086] In one embodiment of the present application, the present invention artificially divides the positive electrode material layer of the positive electrode sheet of the all-solid-state battery into multiple sublayers, preferably 5 layers, along the direction from close to the positive electrode current collector to away from the positive electrode current collector, and the binder content between adjacent sublayers satisfies the above relationship I. The peeling force between adjacent sublayers satisfies the above relationship II.
[0087] As an example, the present invention divides the positive electrode material layer into 5 layers along the direction from close to the positive electrode current collector to away from the positive electrode current collector, namely, the first positive electrode sublayer, the second positive electrode sublayer, the third positive electrode sublayer, the fourth positive electrode sublayer, and the fifth positive electrode sublayer. Preferably, the binder content of the first positive electrode sublayer is 0.25 wt% to 0.45 wt%; the binder content of the second positive electrode sublayer is 0.45 wt% to 0.75 wt%; the binder content of the third positive electrode sublayer is 0.6 wt% to 1.0 wt%; the binder content of the fourth positive electrode sublayer is 0.75 wt% to 1.3 wt%; and the binder content of the fifth positive electrode sublayer is 0.9 wt% to 1.6 wt%.
[0088] In one embodiment of the present application, the present invention prepares an all-solid-state battery positive electrode sheet by a one-step method, and the binder content thereof increases linearly from close to the positive electrode current collector to far away from the positive electrode current collector, and there is no boundary line where the binder content increases sharply on the cross section of the positive electrode material layer. This design can make the interface durability of each component inside the all-solid-state battery positive electrode sheet the same throughout the thickness, thereby improving the consistency of the positive electrode, and further improving the capacity and cycle performance of the all-solid-state battery.
[0089] The present invention also provides an all-solid-state battery, comprising the all-solid-state battery positive electrode sheet as described above, or, comprising the all-solid-state battery positive electrode sheet prepared according to the above preparation method.
[0090] In one embodiment of the present application, the all-solid-state battery of the present invention further includes a negative electrode and a solid electrolyte.
[0091] In one embodiment of the present application, the active material of the negative electrode is selected from graphite materials, silicon materials or a composite material composed of the two.
[0092] Further preferably, the graphite material includes but is not limited to natural graphite, such as block graphite, flake graphite, earthy graphite, etc.; artificial graphite, such as single crystal graphite, polycrystalline graphite, pyrolytic graphite, graphite fiber, etc.
[0093] Further preferably, the silicon material includes but is not limited to crystalline silicon, amorphous silicon and organic silicon.
[0094] In one embodiment of the present application, the active material of the negative electrode may be indium, lithium, aluminum, or an alloy of at least two of the above metals.
[0095] In one embodiment of the present application, the solid electrolyte layer component is solid electrolyte powder, and the type of solid electrolyte is one or more of oxide solid electrolyte, sulfide solid electrolyte and halide solid electrolyte.
[0096] The present invention is described in detail below by specific examples. It should also be understood that the following examples are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0097] Example 1
[0098] In a first aspect, the present embodiment provides an all-solid-state battery positive electrode sheet including a positive electrode current collector (carbon-coated aluminum foil) and a positive electrode material layer formed on the surface of the positive electrode current collector, wherein the positive electrode material layer includes a binder (polyvinylidene fluoride PVDF), a solid electrolyte (Li6PS5Cl), a conductive agent (super p and VGCF), a positive electrode active material (LiNi 0.8 Co 0.1 Mn 0.1 O2), where
[0099] The above PVDF comes from Arkema, the model is Film 302 PGM TR, the molecular weight is 600000 Da, and the viscosity is 3500 mPa·S.
[0100] In this embodiment, LiNi 0.8 Co 0.1 Mn 0.1 The mass ratio of O2, Li6PS5Cl, super p, VGCF and PVDF is 68:24:5:3.
[0101] In this embodiment, the mass ratio of PVDF to the positive electrode material layer is 3:100.
[0102] The preparation method of the positive electrode sheet of the all-solid-state battery in this embodiment is as follows:
[0103] (1) Dissolve 1 g of PVDF in 9 g of butyl butyrate solvent to obtain PVDF glue;
[0104] 1 g LiNi 0.8 Co 0.1 Mn 0.1O2, 0.353 g Li6PS5Cl, 0.037 g super p, 0.037 g VGCF, 0.441 g PVDF glue and 0.511 g butyl butyrate solvent were mixed in a glove box at 2000 rpm for 10 min using a high-speed stirrer, and then defoamed at 500 rpm for 5 min to form a positive electrode slurry with a solid content of 60 wt%;
[0105] (2) Use a scraper to coat the positive electrode slurry on the carbon-coated aluminum foil, quickly transfer it to a vacuum state, and dry it at 130°C for 12 h to form a positive electrode material layer. The surface capacity is 5 mAh / cm 2 All-solid-state battery positive electrode.
[0106] In this embodiment, the vapor pressure of the butyl butyrate solvent is 1.73 kPa, and the polarity parameter is 4.
[0107] A second aspect of this embodiment provides an all-solid-state battery, comprising the above-mentioned all-solid-state battery positive electrode sheet, negative electrode, and solid electrolyte layer.
[0108] In this embodiment, the negative electrode is a lithium-indium alloy sheet (diameter φ=10 mm).
[0109] In this embodiment, the composition of the solid electrolyte layer is Li6PS5Cl.
[0110] The preparation method of the all-solid-state battery of this embodiment is as follows:
[0111] (1) 1000 mg of Li6PS5Cl powder was placed in a mold with a diameter of 10 mm and pressurized to 100 MPa to obtain a solid electrolyte layer;
[0112] (2) The above-mentioned all-solid-state battery positive electrode sheet and lithium-indium alloy sheet are placed on both sides of the solid electrolyte layer in turn for assembly. After assembly, the pressure is increased to 100 MPa, and the nut at the top of the column is tightened to maintain a constant pressure to obtain an all-solid-state battery.
[0113] In this embodiment, the assembly process is completed in a glove box with an argon atmosphere, and the diameters of the above-mentioned all-solid-state battery positive electrode sheet and the lithium-indium alloy sheet are both 10 mm.
[0114] Example 2
[0115] The difference between this embodiment and embodiment 1 is that:
[0116] The mass ratio of PVDF to the positive electrode material layer is 4:100.
[0117] Example 3
[0118] The difference between this embodiment and embodiment 1 is that:
[0119] The mass ratio of PVDF to the positive electrode material layer is 5:100.
[0120] Example 4
[0121] The difference between this embodiment and embodiment 1 is that:
[0122] The positive electrode slurry was coated on the carbon-coated aluminum foil with a scraper, quickly transferred to a vacuum state, and dried at 120° C. for 12 h to prepare a positive electrode material layer.
[0123] Example 5
[0124] The difference between this embodiment and embodiment 1 is that:
[0125] The positive electrode slurry was coated on the carbon-coated aluminum foil with a scraper, quickly transferred to a vacuum state, and dried at 150° C. for 12 h to prepare a positive electrode material layer.
[0126] Example 6 to Example 14
[0127] The difference between the above embodiment and embodiment 1 is that, according to the method of embodiment 1, the materials shown in the following Table 2 are used to prepare the positive electrode sheet of the all-solid-state battery and the all-solid-state battery.
[0128] Table 2
[0129]
[0130] Comparative Example 1
[0131] The difference between this comparative example and Example 1 is:
[0132] The mass ratio of PVDF to the positive electrode material layer is 2:100.
[0133] Comparative Example 2
[0134] The difference between this comparative example and Example 1 is:
[0135] The mass ratio of PVDF to the positive electrode material layer is 7:100.
[0136] Comparative Example 3
[0137] The difference between this comparative example and Example 1 is:
[0138] The positive electrode slurry was coated on the carbon-coated aluminum foil with a scraper, quickly transferred to a vacuum state, and dried at 80° C. for 12 h to prepare a positive electrode material layer.
[0139] Comparative Example 4
[0140] The difference between this comparative example and Example 1 is:
[0141] The positive electrode slurry was coated on the carbon-coated aluminum foil with a scraper, quickly transferred to a vacuum state, and dried at 180° C. for 12 h to prepare a positive electrode material layer.
[0142] Comparative Example 5
[0143] The difference between this comparative example and Example 1 is:
[0144] The all-solid-state battery positive electrode sheet includes a first all-solid-state battery positive electrode layer and a second all-solid-state battery positive electrode layer.
[0145] The first all-solid-state battery cathode layer LiNi 0.8 Co 0.1 Mn 0.1 The mass ratio of O2, Li6PS5Cl, super p, VGCF and PVDF is 68:24:5:2.
[0146] The second all-solid-state battery positive electrode layer LiNi 0.8 Co 0.1 Mn 0.1 The mass ratio of O2, Li6PS5Cl, super p, VGCF and PVDF is 68:24:5:4.
[0147] The preparation method of the positive electrode sheet of the all-solid-state battery is as follows:
[0148] (1) Dissolve 1 g of PVDF in 9 g of butyl butyrate solvent to obtain PVDF glue;
[0149] 1 g LiNi 0.8 Co 0.1 Mn 0.1 O2, 0.353 g Li6PS5Cl, 0.037 g super p, 0.037 g VGCF, 0.294 g PVDF glue and 0.716 g butyl butyrate solvent were mixed with a high-speed stirrer at 2000 rpm for 10 min in a glove box, and then defoamed at 500 rpm for 5 min to form a first positive electrode slurry with a solid content of 60 wt%;
[0150] (2) Using a scraper to coat the first positive electrode slurry on the carbon-coated aluminum foil, quickly transfer it to a vacuum state, and dry it at 130°C for 12 h to prepare the first all-solid-state battery positive electrode layer;
[0151] (3) 1 g LiNi 0.8 Co 0.1 Mn 0.1O2, 0.353 g Li6PS5Cl, 0.037 g super p, 0.037 g VGCF, 0.588 g PVDF glue and 0.452 g butyl butyrate solvent were mixed in a glove box at 2000 rpm for 10 min with a high-speed stirrer, and then defoamed at 500 rpm for 5 min to form a second cathode slurry with a solid content of 60 wt%;
[0152] (4) Use a scraper to coat the second positive electrode slurry on the first all-solid-state battery positive electrode layer, quickly transfer it to a vacuum state, and dry it at 80°C for 12 h to prepare the second all-solid-state battery positive electrode layer, and obtain a surface capacity of 5 mAh / cm 2 All-solid-state battery positive electrode.
[0153] Comparative Example 6
[0154] The difference between this comparative example and Example 1 is:
[0155] The organic solvent is NMP (N-methylpyrrolidone) with a vapor pressure of 0.1 kPa and a polarity parameter of 6.7.
[0156] Comparative Example 7
[0157] The difference between this comparative example and Example 1 is:
[0158] The binder is polyacrylonitrile with a molecular weight of 150,000 Da and a viscosity of 2100 mPa·S.
[0159] Performance Testing
[0160] Binder content: The binder content of the all-solid-state batteries of Examples 1 to 14 and Comparative Examples 1 to 7 was measured, and it was determined whether it changed linearly. The results are shown in Table 3. The determination method and the determination method are as follows:
[0161] By using the energy dispersive X-ray spectrometer (EDS) on a scanning electron microscope (SEM) to observe the cross section of the positive electrode sheet of the all-solid-state battery, the distribution of the PVDF binder can be observed from the F element mapping line scanning analysis diagram on the EDS. Specifically, 50 horizontal lines are taken in the cross section, and the F element distribution on each horizontal line is first scanned and analyzed using EDS to determine whether the PVDF binder content of each sub-layer meets -0.05≤X a +0.23- X b ≤0.05. If it is satisfied, it is recorded as “yes” that the PVDF content in the electrode section changes linearly, otherwise it is recorded as “no”.
[0162] Peeling force: The peeling force of the all-solid-state batteries of Examples 1 to 14 and Comparative Examples 1 to 7 was measured, and the results are shown in Table 3. The measurement method is as follows:
[0163] The 180° peeling method is used to quantitatively measure the peeling strength, i.e. the peeling force. The free end of the positive electrode sheet is folded 180°, and the free end of the positive electrode sheet and the test plate are clamped on the upper and lower clamps respectively. In the same environment, a tensile tester is used to perform continuous peeling until the positive electrode collector and the positive electrode material layer are completely separated. The peeling strength value can be directly read to obtain the peeling force between the positive electrode material layer and the positive electrode collector.
[0164] For the peeling force of the positive electrode material layer at different thickness positions, argon ion milling was used to obtain the first positive electrode sublayer, the second positive electrode sublayer, the third positive electrode sublayer, the fourth positive electrode sublayer and the fifth positive electrode sublayer, and then their peeling force was tested. Take the electrode sheet, cut it into 2.5 cm × 25 cm strips, stick the double-sided tape on the steel plate, and use the roller to go back and forth 3 times to make the double-sided tape and the steel plate stick tightly; then use the double-sided tape to stick the cut electrode strips to the steel plate, and use the roller to go back and forth 3 times to make them stick tightly; fix the steel plate on the peeling tester so that the electrode and the peeling direction are always controlled at 90°, perform the peeling force test, and read the data. And observe whether the peeling force of each sublayer from close to the positive current collector to away from the positive current collector satisfies -1≤Y a +1.5- Y b ≤1, if it is satisfied, it is recorded as “yes” that the peeling force of each positive electrode sub-layer of the electrode sheet is linearly distributed, otherwise it is recorded as “no”.
[0165] Normal temperature cycle test: The all-solid-state batteries of Examples 1 to 14 and Comparative Examples 1 to 7 were subjected to normal temperature cycle tests, and the results are shown in Table 3. The determination method is as follows:
[0166] Under 25°C environment, the all-solid-state batteries of Examples 1 to 5, 7 to 14 and Comparative Examples 1 to 7 were subjected to long-cycle charge and discharge after being capacitated, and the number of normal temperature cycles was measured; the test conditions were to conduct long-cycle charge and discharge tests on the batteries after they were capacitated, and during the process, the first-cycle capacitated discharge specific capacity and the number of normal temperature cycles when the SOH was 80% were recorded; the operating voltage range was 1.9 V ~3.7 V, the capacitated ratio was 0.1 C, and the normal temperature cycle test ratio was 0.3 C.
[0167] For Example 6, the testing method is the same as that of the other examples and comparative examples, except that the operating voltage range is 1.4 V to 4.25 V.
[0168] The experimental data and analysis are as follows:
[0169] Table 3 All-solid-state battery performance test results of Examples 1 to 14 and Comparative Examples 1 to 7
[0170]
[0171] It can be seen from the data of Examples 1-3, Examples 7-14 and Comparative Examples 1-2 that when the preparation method of the present invention is adopted, especially when the mass ratio of the binder to the positive electrode material layer is (3-5):100, and the binder content in the prepared positive electrode sheet of the all-solid-state battery increases gradually, it can effectively improve the performance of the all-solid-state battery.
[0172] When the mass ratio of the binder to the positive electrode material layer is not within the above range, for Comparative Example 1, the binder content is low, and the binder floats under high-temperature vacuum heating conditions, causing the active material to fall off the positive electrode current collector. Severely powdered all-solid-state battery positive electrode sheets cannot be used to prepare all-solid-state batteries.
[0173] For Comparative Example 2, the binder content is high, which causes the electron and ion pathways in the positive electrode of the all-solid-state battery to be blocked, thereby deteriorating the battery performance.
[0174] It can be seen from the data of Examples 4 to 5 and Comparative Examples 3 to 4 that when the preparation method of the present invention is adopted, especially when the drying temperature is 120°C to 150°C, and the binder content in the prepared all-solid-state battery positive electrode sheet increases gradually, it can effectively improve the performance of the all-solid-state battery.
[0175] When the drying temperature during the preparation of the positive electrode sheet of the all-solid-state battery is not within the above range, for Comparative Example 3, its lower drying temperature cannot make the binder linearly distributed, and the interface durability of the positive electrode sheet of the all-solid-state battery close to the negative electrode side is worse than that of the positive electrode sheet of the all-solid-state battery close to the positive electrode collector side, resulting in easy interface debonding of the components inside the positive electrode sheet of the all-solid-state battery close to the negative electrode side, thereby worsening the interface contact and affecting the battery performance.
[0176] For Comparative Example 4, its higher drying temperature causes the binder to float up very quickly, resulting in too low a binder content near the positive current collector side, leading to poor adhesion between the positive current collector and the active material, thus causing the positive electrode membrane of the all-solid-state battery to fall off, making it impossible to prepare an all-solid-state battery.
[0177] It can be seen from the data of Example 6 that when the preparation method of the present invention is adopted and the binder content in the prepared all-solid-state battery positive electrode sheet increases gradually, even if the high-voltage positive electrode LNMO is used as the positive electrode active material, the prepared all-solid-state battery also has good cycle performance.
[0178] It can be seen from the data of Example 1 and Comparative Example 5 that the use of an all-solid-state battery positive electrode sheet in which the binder content is linearly increased from the direction close to the positive electrode collector to the direction away from the positive electrode collector can avoid the problem of transition of PVDF content in the cross section of the electrode sheet; the present invention can prepare an all-solid-state battery positive electrode sheet with a gradient distribution of binder content in one step, the process operation is simple, and the production cost is reduced.
[0179] For Comparative Example 5, the binder contents in the two positive electrode material layers are different, and the interface impedance between the two positive electrode material layers will increase due to the transition of the binder content, hindering the transmission of lithium ions and causing the performance of the all-solid-state battery to decrease. At the same time, the preparation process requires a two-step coating process, which is time-consuming and inefficient.
[0180] It can be seen from the data of Comparative Examples 6 and 7 that when the molecular weight and viscosity of the organic solvent and binder are not within the specified range of the present invention, the performance of the all-solid-state battery deteriorates. This is because the highly polar NMP solvent will induce the decomposition of the solid electrolyte, and the lower vapor pressure of NMP prevents its binder from being linearly distributed; the lower molecular weight of polyacrylonitrile makes its bonding effect poor, and its lower viscosity will cause the components such as the positive electrode active material and the solid electrolyte to settle during the pulping process, affecting the consistency, thereby reducing the reliability and safety of the all-solid-state battery.
[0181] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A positive electrode sheet for an all-solid-state battery, comprising a positive electrode current collector and a positive electrode material layer formed on the surface of the positive electrode current collector, wherein the positive electrode material layer comprises a binder, characterized in that: The positive electrode material layer includes a positive electrode first sublayer and a positive electrode second sublayer, and the positive electrode first sublayer is located between the positive electrode current collector and the positive electrode second sublayer; When the thickness of the positive electrode sheet is H μm, the thickness of the positive electrode first sublayer and the positive electrode second sublayer is 0.2H μm, and the binder content of the positive electrode first sublayer is X a wt%, the binder content of the second positive electrode sublayer is X b wt%, the positive electrode sheet satisfies the following relational formula I: -0 .05≤X a +0 .23-X b ≤0 .05; The binder content of the positive electrode material layer satisfies the following conditions (a) and (b): (a) the mass ratio of the binder to the positive electrode material layer is (3-5):100; (b) the content of the binder is distributed in an increasing manner from close to the positive electrode current collector to away from the positive electrode current collector; The method for preparing the positive electrode sheet of the all-solid-state battery comprises the following steps: (1) Preparing positive electrode slurry: dissolving the binder in an organic solvent to obtain a binder paste; The binder glue and the positive electrode material composition are mixed to obtain the positive electrode slurry, wherein: The molecular weight of the binder is 500000 Da~1200000 Da, and the viscosity of the binder is 3000 mPa·S~3500 mPa·S; The organic solvent has a vapor pressure of 1.5 kPa to 3 kPa and a polarity parameter of 0 to 4.5; (2) coating the positive electrode slurry on the surface of the positive electrode current collector, drying, and preparing a positive electrode material layer to obtain the positive electrode sheet of the all-solid-state battery, wherein: The drying temperature is 120℃~150℃.
2. The all-solid-state battery positive electrode sheet according to claim 1, characterized in that: The range of H is 50 μm≤H≤300 μm.
3. The all-solid-state battery positive electrode sheet according to claim 1, characterized in that: The peeling force of the first sublayer of the positive electrode is Y a N / m, the peeling force of the second sublayer of the positive electrode is Y b N / m, the positive electrode sheet satisfies the following relationship II: -1≤Y a +1.5- And b ≤1。 4. The all-solid-state battery positive electrode sheet according to claim 1, characterized in that: The positive electrode first sublayer and the positive electrode second sublayer are adjacent sublayers.
5. The all-solid-state battery positive electrode sheet according to claim 1, characterized in that: The positive electrode material layer further comprises a solid electrolyte, a positive electrode active material and a conductive agent, wherein the solid electrolyte is selected from at least one of an oxide solid electrolyte, a sulfide solid electrolyte and a halide solid electrolyte; The positive electrode active material is selected from at least one of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide and lithium-rich manganese-based oxide; The conductive agent is selected from at least one of graphite, graphene, carbon black, carbon fiber and carbon nanotubes; The binder is selected from at least one of styrene-butadiene rubber, sodium alginate, polyacrylonitrile, polyurethane, polyacrylic acid, ethylene-propylene-diene monomer, styrene-butadiene rubber, polyvinyl methacrylate glycerol methacrylate copolymer, hydrogenated nitrile rubber, nitrile rubber, poly(acrylic acid-poly(ethylene glycol) methyl ether methacrylate) copolymer, polyvinylidene fluoride and polyvinylidene fluoride copolymer.
6. A method for preparing a positive electrode sheet of an all-solid-state battery, characterized in that: The following steps are involved: (1) Preparing positive electrode slurry: dissolving the binder in an organic solvent to obtain a binder paste; The binder glue and the positive electrode material composition are mixed to obtain the positive electrode slurry, wherein: The molecular weight of the binder is 500000 Da~1200000 Da, and the viscosity of the binder is 3000 mPa·S~3500 mPa·S; The organic solvent has a vapor pressure of 1.5 kPa to 3 kPa and a polarity parameter of 0 to 4.5; (2) coating the positive electrode slurry on the surface of the positive electrode current collector, drying, and preparing a positive electrode material layer to obtain the positive electrode sheet of the all-solid-state battery, wherein: The drying temperature is 120℃~150℃; The mass ratio of the binder to the positive electrode material layer is (3-5):100; The positive electrode material layer includes a positive electrode first sublayer and a positive electrode second sublayer, and the positive electrode first sublayer is located between the positive electrode current collector and the positive electrode second sublayer; When the thickness of the positive electrode sheet is H μm, the thickness of the positive electrode first sublayer and the positive electrode second sublayer is 0.2H μm, and the binder content of the positive electrode first sublayer is X a wt%, the binder content of the second positive electrode sublayer is X b wt%, the positive electrode sheet satisfies the following relational formula I: -0 .05≤X a +0 .23-X b ≤0 .05; The binder content of the positive electrode material layer is distributed in an increasing manner from close to the positive electrode current collector to far away from the positive electrode current collector.
7. The preparation method according to claim 6, characterized in that: In the step (1), the positive electrode material composition includes a positive electrode active material, a solid electrolyte and a conductive agent.
8. An all-solid-state battery, characterized in that: It includes the all-solid-state battery positive electrode sheet as described in any one of claims 1 to 5, or, it includes the all-solid-state battery positive electrode sheet prepared by the preparation method according to any one of claims 6 to 7.
Citation Information
Patent Citations
Preparation method of multi-layer coating pole piece
CN111370649A
Positive electrode and electrochemical device comprising same
CN113782708A
Lithium ion battery positive plate and lithium ion battery
CN116435466A
Integrated sulfide all-solid-state battery electrode plate and preparation method thereof
CN116864624A
Positive plate and battery comprising same
CN116960332A
Cited By
Solid-state battery and production and preparation method of solid-state battery
CN121331852A
All-solid-state battery and consistency test method thereof
CN122225056A