Creep aging forming method for high-ribbed thin-walled components

By determining the relationship between creep forming temperature and bending stress, setting target forming conditions, and processing highly reinforced thin-walled components in an autoclave, the problem of creep microcracks is solved and high-quality forming of highly reinforced thin-walled components is achieved.

CN118595271BActive Publication Date: 2024-10-18CENT SOUTH UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411081286.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-10-18
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

Highly reinforced thin-walled components are prone to creep microcracks during the creep aging forming process, leading to manufacturing defects.

Method used

By determining the first mapping relationship between creep forming temperature, bending stress and fracture duration, setting the target forming temperature and target bending stress, and performing creep aging treatment in the autoclave to reduce the bending stress of the high-reinforced wall plate blank, specifically The steps include sealing the vacuum bag, increasing the pressure and temperature of the autoclave, and releasing part of the air pressure at high temperatures to reduce bending stress.

Benefits of technology

It effectively avoids the occurrence of creep microcracks and obtains high-reinforced thin-walled components with no surface defects and high quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118595271B_ABST
    Figure CN118595271B_ABST
Patent Text Reader

Abstract

The present invention provides a creep aging forming method for high-ribbed thin-walled components. The forming method comprises the following steps: vacuum loading a high-ribbed wall panel blank. According to a first mapping relationship among creep forming temperature, bending stress and fracture time of the corresponding material of the high-ribbed wall panel blank, a target forming temperature and a corresponding target bending stress are determined. The internal stress distribution of the high-ribbed wall panel blank after loading is simulated to determine the second air pressure corresponding to the high-ribbed wall panel blank under the target bending stress. The wall panel mold sealing structure is placed in an autoclave, the pressure in the tank is first increased to the first air pressure and then released to the second air pressure, and creep aging forming is performed under the conditions of the target forming temperature and the corresponding forming time. The high-ribbed wall panel blank is subjected to a small bending stress, so that after creep aging deformation, no creep microcracks will appear, thereby obtaining a high-ribbed thin-walled component with no surface defects and high quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal high-rib component processing, in particular to a creep aging forming method for high-rib thin-wall components. Background Art

[0002] Large high-rib panel structures are widely used in key structures in the fields of aerospace, weapons and equipment due to their advantages such as high structural efficiency and strong bearing capacity, such as aircraft high-rib wing panels. Therefore, high-performance and high-precision manufacturing of high-rib panel structures is extremely important. The creep aging forming process is an advanced manufacturing technology that is particularly suitable for the forming of large thin-walled components. The components can be formed and formed under the same temperature field and stress field conditions, and have the advantages of good repeatability, low residual stress, and good performance. However, with the improvement of carrying capacity, high-rib structures are further developed towards the characteristics of large rib height-to-thickness ratio, thin wall with weak stiffness, and complex large curvature. Such components face manufacturing defects such as creep microcracks under the extreme conditions of high temperature, high stress, and high pressure loads during creep aging forming. Summary of the invention

[0003] The main purpose of the present invention is to provide a creep aging forming method for high-ribbed thin-walled components to solve the technical problem of creep microcracks occurring during creep aging forming of high-ribbed thin-walled components.

[0004] To achieve the above object, the present invention provides a creep aging forming method for high-rib thin-walled components, comprising the following steps:

[0005] The high-rib wall panel blank and the mold are sealed by a vacuum bag, and vacuum is drawn so that the high-rib wall panel blank is bent and deformed to contact the mold, thereby obtaining a wall panel mold sealing structure.

[0006] According to the first mapping relationship among the creep forming temperature, bending stress and fracture time of the material corresponding to the high-ribbed wall panel blank, the target forming temperature and the corresponding target bending stress are determined. The target forming temperature is selected from the optional forming temperature range of the high-ribbed wall panel blank, and the forming time corresponding to the target forming temperature is less than the fracture time corresponding to the target forming temperature in the first mapping relationship.

[0007] The internal stress distribution of the high-ribbed wall panel blank after loading is simulated to determine the second air pressure corresponding to the high-ribbed wall panel blank under the target bending stress.

[0008] The wall panel mold sealing structure is placed in an autoclave, and the pressure and temperature are increased to perform creep aging treatment to obtain a high-rib thin-wall component. The process of increasing the pressure includes: increasing the pressure to a first pressure, releasing the pressure to a second pressure, and then maintaining the second pressure. The target temperature of the increased temperature is the target forming temperature.

[0009] According to an embodiment of the present application, the step of determining a first mapping relationship among the creep forming temperature, the bending stress and the fracture time comprises:

[0010] The material corresponding to the high-rib wall panel blank is subjected to a material creep rupture experiment under conditions of different creep forming temperatures and different bending stresses, and a creep forming temperature-bending stress-rupture time relationship diagram is drawn to obtain the first mapping relationship.

[0011] According to the implementation manner of the present application, the step of simulating the internal stress distribution of the high-ribbed wall panel blank after loading to determine the second air pressure corresponding to the high-ribbed wall panel blank under the target bending stress includes:

[0012] A simulation model of internal stress distribution of high-rib wall panel blank after loading is established.

[0013] An internal stress distribution cloud map is calculated according to the simulation model, and a second air pressure corresponding to the high-rib wall panel blank under the target bending stress is determined based on the internal stress distribution cloud map.

[0014] According to the implementation of the present application, the steps of establishing a simulation model of the internal stress distribution of the high-rib wall panel blank after loading include:

[0015] The high-ribbed wall panel blank is meshed by finite element units, and material properties are assigned to the high-ribbed wall panel blank. Symmetrical constraints and linear air pressure loading boundary conditions are applied to obtain the simulation model.

[0016] According to an embodiment of the present application, the step of determining the optional forming temperature range includes:

[0017] The material constitutive equation of the high-ribbed wall panel blank was fitted until the error between the fitted creep curve and the experimental creep curve was less than 5%, and the fitted constitutive equation was obtained.

[0018] Based on the fitted constitutive equation, the creep aging forming of the high-rib wall panel blank is simulated to obtain an optional forming temperature range and a corresponding optional forming time.

[0019] According to an embodiment of the present application, the optional forming temperature range is 120~200°C, and the target forming temperature is 155~165°C.

[0020] According to an embodiment of the present application, in the step of increasing the pressure to the first pressure, the pressure increase rate is 20-50 kPa / min. In the step of increasing the temperature, the temperature increase rate is 1-3°C / min.

[0021] According to an embodiment of the present application, the speed of releasing the air pressure is 20~50kPa / min.

[0022] According to an embodiment of the present application, the first air pressure ranges from 1.5 to 2.0 MPa, and the second air pressure ranges from 0.3 to 0.5 MPa.

[0023] According to an embodiment of the present application, the material of the high-rib wall panel blank is aluminum alloy.

[0024] In the above-mentioned creep aging forming method for high-ribbed thin-walled components, a reasonable target forming temperature and a corresponding target bending stress are determined according to the first mapping relationship among creep forming temperature, bending stress and fracture time, and then the pressure of the autoclave is released based on the target bending stress. At this time, the high-ribbed wall plate blank is subjected to a small bending stress, so that after creep aging deformation, no creep microcracks will appear, thereby obtaining a high-ribbed thin-walled component with no surface defects and high quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0026] Figure 1 This is a stress distribution diagram of a high-rib structure and its cross section after bending loading in one embodiment of the present application;

[0027] Figure 2 It is a schematic diagram of a typical creep curve of a metal;

[0028] Figure 3 It is a schematic diagram of grain boundary holes in materials during creep under high stress or high temperature conditions;

[0029] Figure 4 This is a flow chart of a creep aging forming method for high-ribbed thin-walled components according to an embodiment of the present application;

[0030] Figure 5a This is a stress distribution diagram of a high-ribbed thin-walled component under 2.0 MPa according to an embodiment of the present application;

[0031] Figure 5b This is a stress distribution diagram of a high-ribbed thin-walled component under 0.3 MPa according to an embodiment of the present application;

[0032] Figure 5c This is a diagram of the stress evolution of the high ribs according to an embodiment of the present application;

[0033] Figure 6a is a schematic diagram of increased pressure and temperature according to one embodiment of the present application;

[0034] Figure 6b It is a schematic diagram of stress evolution of a high-rib component during creep aging treatment in one embodiment of the present application;

[0035] Figure 7 The high-ribbed thin-walled component of Example 1 of the present application is sprayed with a developer and a partial enlarged photo; wherein a is a photo of the real object; b is a partial enlarged photo shown in the rectangular dotted frame in a;

[0036] Figure 8 It is the real object and partial enlarged photo of the high-ribbed thin-walled component after spraying the developer in comparative example 1 of the present application; among them, a is the real object photo; b is the partial enlarged photo shown in the rectangular dotted frame in a.

[0037] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0038] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0040] In addition, in the present invention, the descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0041] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0042] The present invention provides a creep aging forming method for a high-rib thin-wall component, comprising the following steps:

[0043] S100: The high-rib wall panel blank and the mold are sealed by a vacuum bag, and vacuum is drawn so that the high-rib wall panel blank is bent and deformed to contact the mold, thereby obtaining a wall panel mold sealing structure.

[0044] High-rib thin-wall components, or high-rib panels, are structural components made from a whole thick plate blank. They are characterized by criss-crossing ribs on the skin, and the height of the ribs is generally greater than 30mm. This panel structure is widely used in aircraft parts such as wings, fuselages, and tails.

[0045] Creep Age Forming (CAF) is a forming process that combines creep deformation of materials with artificial aging strengthening. It is mainly used to prepare large thin-walled structural parts such as aluminum alloys. The basic principle of creep age forming is to use the creep deformation and aging strengthening phenomenon of metals under specific temperature and stress conditions.

[0046] Creep aging forming includes a loading stage, a creep aging stage and an unloading stage. Step S100 is a vacuum loading stage.

[0047] During the loading stage, the flat panel blank is first placed on the mold and the vacuum bag is sealed, and then the vacuum is evacuated. At this time, the high-ribbed panel blank gradually bends toward the mold surface. According to material mechanics, the stress on the ribs gradually increases during the bending process of the high-ribbed panel blank, and the stress at the top of the rib is the largest and exceeds the yield strength.

[0048] After the high-ribbed siding blank is vacuumed, bent and loaded, and the outer surface is close to the mold surface, it enters the autoclave as a whole and begins to increase pressure and temperature. When it reaches the target temperature of 120-200°C, it enters the insulation stage and produces creep deformation. The specific process is as follows: After vacuuming, the high-ribbed siding blank and the mold together with the vacuum bag (siding mold sealing structure) enter the autoclave equipment as a whole. The autoclave equipment begins to increase pressure and temperature until the target temperature. At this time, the ribs are further bent to fit the mold surface, the internal stress on the ribs is also greater, and more areas exceed the yield strength, such as Figure 1 As shown, the skin is relatively thin and has less internal stress.

[0049] Creep is a slow and irreversible deformation behavior of metal materials under certain temperature and external load conditions, which goes through initial transient creep, steady-state creep and accelerated creep stages. Figure 2 As shown, the whole process is related to three important process parameters: internal stress level, temperature and time, and the creep deformation of the material is positively correlated with the above three process parameters.

[0050] The study found that for high-ribbed wall structures, the bending internal stress level on the ribs is large after loading, exceeding the yield strength. Under long-term high temperature conditions, the internal stress has no time to decay, resulting in the formation of holes between the grain structures of the ribs. Under the action of external loads, the holes on the grain boundaries gradually grow and aggregate, and eventually connect together, such as Figure 3 As shown, creep microcracks occur in local high stress areas.

[0051] Therefore, this application proposes to reduce the risk of microcracks in high-rib components by lowering the creep temperature and internal stress level. The specific idea is that the high stress creep on the high ribs of the component is maintained for a shorter time than the creep rupture time of the high stress at the forming temperature.

[0052] S200: Determine a target forming temperature and a corresponding target bending stress according to a first mapping relationship among the creep forming temperature, bending stress and fracture time of the material corresponding to the high-ribbed wall panel blank, wherein the target forming temperature is selected from an optional forming temperature range of the high-ribbed wall panel blank, and the forming time corresponding to the target forming temperature is less than the fracture time corresponding to the target forming temperature in the first mapping relationship.

[0053] There is a corresponding mapping relationship between the creep forming temperature, bending stress and fracture time of the material. The mapping relationship between the three in the high-ribbed wall panel blank is called the first mapping relationship. The method of obtaining the first mapping relationship is not specifically limited, and it can be obtained through specific experiments, such as processing the material corresponding to the high-ribbed wall panel blank into a small sample and then placing it on the equipment for creep testing to obtain the fracture time, or it can be obtained through simulation experiments.

[0054] The first mapping relationship includes the fracture durations of multiple creep forming temperatures under different bending stresses. The bending stress is the bending stress borne by the high-ribbed wallboard blank. The fracture duration is the duration of the material corresponding to the high-ribbed wallboard blank to fracture at the corresponding creep forming temperature.

[0055] The target forming temperature is the target creep forming temperature controlled by the high-ribbed wall panel blank during the creep aging stage, and the target bending stress is the bending stress controlled by the high-ribbed wall panel blank during the creep aging stage.

[0056] The optional forming temperature range and the corresponding forming time are the forming temperature range and forming time selected to meet the general requirements of the high-ribbed wall panel billet in the conventional creep aging stage, that is, the forming temperature range and forming time that meet the creep aging stage requirements of the high-ribbed wall panel billet without considering the creep microcracks of the high-ribbed wall panel billet.

[0057] See also Figure 6b, the target creep forming temperature is selected from the optional forming temperature range, and the selected optional forming temperature must satisfy that the corresponding forming time is less than the fracture time corresponding to the forming temperature in the first mapping relationship. The selected optional forming temperature is the target creep forming temperature. The forming time corresponding to the selected optional forming temperature is the forming time corresponding to the target creep forming temperature.

[0058] Since there may be one or more optional forming temperatures that meet this condition, correspondingly, the target creep forming temperature may also be one or more.

[0059] A high temperature creep test was carried out on a certain grade of high-strength aluminum alloy sample. The test results are shown in Table 1:

[0060] Table 1 Temperature-stress-fracture time relationship

[0061]

[0062] It is found that as the creep temperature increases, the creep rupture time of the material under high stress is advanced. According to the above high temperature-high stress creep rupture time relationship, when setting the creep forming process of high-ribbed wall panels, it is necessary to pay attention to the time when the high stress of the ribs is maintained is less than the rupture time of the high stress at this temperature.

[0063] The first mapping relationship may be in a table form as shown in Table 1, or may be in a form of a fitting formula or curve based on creep forming temperature, bending stress, and fracture time.

[0064] In the first mapping relationship, the creep forming temperature and the bending stress are negatively correlated with the fracture time. If at least one of the creep forming temperature and the bending stress is reduced, the fracture time will be extended.

[0065] In the present application, at least one of the target creep forming temperature and the target bending stress is reduced. Exemplarily, only the target creep forming temperature is reduced. Exemplarily, only the target bending stress is reduced. Exemplarily, both the target creep forming temperature and the target bending stress are reduced.

[0066] S300: Simulate the internal stress distribution of the high-ribbed wall panel blank after loading to determine the second air pressure corresponding to the high-ribbed wall panel blank under the target bending stress.

[0067] The high-rib wall panel blank and the mold enter the autoclave equipment, and the equipment begins to increase the pressure and temperature until the target pressure and target temperature are reached. Figure 5a and Figure 5b, the high-ribbed wall panel blank is further subjected to increased pressure, the internal stress on the ribs is also greater, and more areas exceed the yield strength. Therefore, it is necessary to adjust the target pressure of the autoclave (i.e., the second air pressure) to reduce the air pressure load of the high-ribbed wall panel blank, in order to reduce the bending stress of the high-ribbed wall panel blank.

[0068] The bending stress of the high-rib wall panel blank after vacuum loading is also corresponding to the corresponding air pressure. Therefore, based on the internal stress distribution simulation model, according to the initial stress (i.e. target bending stress) to determine the corresponding air pressure (Second air pressure).

[0069] The specific analysis process can include the following processes: Determine the loading of the high-ribbed wall panel through finite element simulation The highest initial stress on the rib after air pressure (i.e. first air pressure) loading (i.e. initial bending stress), according to the first mapping relationship above, it can be determined that the highest initial stress at this time is The fracture occurs at the creep forming temperature for a short time, and the finite element method is used to further study the pressure load of the wall panel from Release to (Second air pressure), again based on the first mapping relationship, the initial stress on the high rib is Whether the time sustained at the creep deformation temperature is within the safe area or the safe area can be reached after a short stress decay process.

[0070] S400: placing the wall panel mold sealing structure in an autoclave, increasing the pressure and temperature to perform creep aging treatment to obtain a high-rib thin-walled component; wherein the process of increasing the pressure includes: increasing the pressure to a first pressure, releasing the pressure to a second pressure, and then maintaining the second pressure; the target temperature of the increased temperature is the target forming temperature.

[0071] In this step, after the pressure in the autoclave is released, the bending pressure borne by the high-rib wall plate blank is the target bending pressure. Creep aging forming is performed according to the above-determined target forming temperature and the corresponding forming time.

[0072] The pressure value of the first air pressure is greater than the pressure value of the second air pressure, so that the high-rib wall panel bends and fits the mold surface, generating the plastic deformation required for forming. The first air pressure is the pressure value selected to meet the general requirements of the high-rib wall panel blank in the conventional creep aging stage, that is, the pressure value that meets the requirements of the creep aging stage of the high-rib wall panel blank without considering the creep microcracks of the high-rib wall panel blank.

[0073] See also Figure 6a and Figure 6bIn general, in order to solve the problem that high stress levels in creep forming of high-rib wall panels are prone to creep microcracks at high temperatures, the present invention proposes a new two-stage variable pressure constant temperature creep aging forming process. On the one hand, by setting a higher autoclave air pressure during the loading stage, the high-rib wall panels are bent to fit the mold surface, generating the plastic deformation required for forming. On the other hand, after the initial air pressure load is applied, part of the air pressure load is immediately released to reduce the high bending stress on the high ribs of the wall panels. The reduced stress level is maintained at the forming temperature for a period of time, and the metal material structure will not have defects such as holes, which solves the problem of local microcracks in creep forming of high-rib wall panels.

[0074] In the above-mentioned creep aging forming method for high-ribbed thin-walled components, a reasonable target forming temperature and a corresponding target bending stress are determined based on the first mapping relationship among creep forming temperature, bending stress and fracture time, and then the air pressure load is released to the autoclave based on the target bending stress. At this time, the high-ribbed wall plate blank is subjected to a small bending stress, so that after creep aging deformation, no creep microcracks will appear, thereby obtaining a high-ribbed thin-walled component with no surface defects and high quality.

[0075] In some embodiments, the step of determining a first mapping relationship among the creep forming temperature, the bending stress and the fracture time comprises:

[0076] The material corresponding to the high-rib wall panel blank is subjected to a material creep rupture experiment under conditions of different creep forming temperatures and different bending stresses, and a creep forming temperature-bending stress-rupture time relationship diagram is drawn to obtain the first mapping relationship.

[0077] By setting different creep forming temperature conditions, illustratively, in the range of 120-200°C, a creep forming temperature is set every 10°C from 120°C, and setting different bending stress conditions, illustratively, the bending stress is set in the range of 300-500MPa. A material creep rupture experiment is carried out under the above different creep forming temperatures and different bending stress conditions, and a creep forming temperature-bending stress-rupture time relationship diagram is drawn based on the experimental data obtained from the above creep rupture experiment.

[0078] Compared with the simulation method, the relationship between creep forming temperature, bending stress and fracture time reflected by the first mapping relationship is closer to the real relationship. The target forming temperature and the corresponding target bending stress determined in this way are also more accurate, and the overall creep aging forming method of high-ribbed thin-walled components is more reliable.

[0079] In some embodiments, the internal stress distribution simulation model is an internal stress distribution cloud map. This method can more intuitively determine the high bending stress area and specific bending stress value of the high-rib wall panel blank.

[0080] In some embodiments, the step of simulating the internal stress distribution of the high-ribbed wall panel blank after loading to determine the second air pressure corresponding to the high-ribbed wall panel blank under the target bending stress includes:

[0081] Establish a simulation model of internal stress distribution of high-ribbed wall panel blank after loading;

[0082] An internal stress distribution cloud map is calculated according to the simulation model, and a second air pressure corresponding to the high-rib wall panel blank under the target bending stress is determined based on the internal stress distribution cloud map.

[0083] In some embodiments, the steps of establishing a simulation model of the internal stress distribution of the high-rib wall panel blank after loading include:

[0084] The high-ribbed wall panel blank is meshed by finite element units, and material properties are assigned to the high-ribbed wall panel blank. Symmetrical constraints and linear air pressure loading boundary conditions are applied to obtain the simulation model.

[0085] In some embodiments, the step of determining the optional forming temperature range includes:

[0086] S310: Fitting the material constitutive equation of the high-ribbed wall panel blank until the error between the fitted creep curve and the experimental creep curve is less than 5%, thereby obtaining the fitted constitutive equation.

[0087] For example, the same material of the high-rib wall panel blank is used for creep aging and basic mechanical property experimental tests to obtain the material creep and mechanical properties under different temperatures and stresses. The creep data at a suitable temperature is used as the original data to construct the material constitutive equation, and the constitutive equation is fitted by mathematical software to ensure that the error between the fitted creep curve and the experimental creep curve is less than 5%.

[0088] Among them, the basic experimental parameters of mechanical properties include yield stress, tensile stress, elongation, hardness, and loading rate. Mathematical software includes MATLAB, Scilab, FreeMat, etc.

[0089] S320: Based on the fitted constitutive equation, the creep aging forming of the high-rib wall panel blank is simulated to obtain an optional forming temperature range and a corresponding optional forming time.

[0090] The material constitutive equation of the high-ribbed wall panel blank can be obtained by querying the data, and the creep aging and mechanical properties basic experimental tests can be carried out on the same material of the high-ribbed wall panel blank to construct the material constitutive equation.

[0091] For example, the fitted constitutive equation is written through a subroutine and then imported into the simulation software to simulate the creep aging forming process of the sheet metal. The process parameters of the high-rib wall blank in the autoclave (such as pressure 0.8-2MPa, temperature 140℃-200℃, duration 0.5-12h) and the mold surface are added as boundary conditions to obtain the preliminary creep aging forming results, and the results are compared with the target surface to obtain the pre-formed area that cannot reach the target surface by creep aging process alone and the underbending or overbending amount that needs to be compensated. Simulation software includes ANSYS, Comsol, Marc, etc.

[0092] In some embodiments, the optional forming temperature range is 120-200° C. The target forming temperature is 155-165° C.

[0093] See also Figure 6b , the difference between t2 and t1 (t2-t1) is the duration of high stress maintenance, t creep rupture is the creep rupture duration, and it is necessary to satisfy t2-t1<t 蠕变断裂 To avoid cracks. In the above-mentioned target forming temperature range, the creep rupture time of the high-rib wall panel blank is relatively long, and in some cases can reach about 5 hours, which is longer than the component forming temperature time at this temperature. And considering that the creep forming process is also a stress relaxation process, the stress level on the high rib will gradually decay in practice, the creep rupture time will be longer, or even no rupture will occur. Therefore, at the target forming temperature, the margin of the safety air pressure corresponding to the creep rupture is relatively large, and the creep aging forming method of the high-rib thin-walled component has better robustness.

[0094] In some more specific embodiments, the target forming temperature is 160°C.

[0095] In some embodiments, in the step of increasing the pressure to the first pressure, the pressure increasing rate is 20-50 kPa / min; in the step of increasing the temperature, the temperature increasing rate is 1-3°C / min.

[0096] Under this condition, see Figure 6a The combination of the pressure increase rate and the temperature increase rate can ensure that when the pressure reaches the first pressure, the temperature in the autoclave is relatively low, further reducing the probability of cracks in high-ribbed thin-walled components.

[0097] In some embodiments, the rate of releasing the gas pressure is 20-50 kPa / min.

[0098] See also Figure 6aOn the one hand, since the autoclave is increasing pressure and temperature, when the pressure in the autoclave reaches the first pressure, the temperature inside the autoclave has reached a certain temperature. Therefore, during the pressure relief process, the pressure relief speed cannot be too slow, otherwise the high-ribbed wall panel blank may stay under a relatively large pressure (the pressure value is between the first pressure and the second pressure) for a long time, and the probability of cracks cannot be reduced to the expected value.

[0099] On the other hand, if the pressure relief speed is too fast, the high-ribbed wall panel blank will recover its elasticity and not fit tightly with the mold, resulting in unqualified dimensions of the prepared high-ribbed thin-walled components.

[0100] Therefore, at the above-mentioned speed of releasing the air pressure, the probability of cracks occurring in the high-ribbed thin-walled component is further reduced, and the product size qualification rate is further improved.

[0101] Furthermore, in some cases, the speed of releasing the gas pressure is combined with the above-mentioned heating speed, so that after the pressure of the autoclave is released to the second pressure, the temperature of the autoclave simultaneously reaches the target forming temperature, or the temperature of the autoclave reaches the target forming temperature in a shorter time.

[0102] In some embodiments, the first air pressure ranges from 1.5 to 2.0 MPa, and the second air pressure ranges from 0.3 to 0.5 MPa.

[0103] Under the condition of the first air pressure, the vacuum bag can make the high-ribbed wall panel blank deform greatly and fit tightly with the mold. The second air pressure range is 0.3~0.5MPa, which can ensure that the high-ribbed wall panel blank is subjected to less bending stress, further reducing the risk of cracks.

[0104] In some embodiments, the material of the high-rib wall panel blank is aluminum alloy, such as a high-strength aluminum alloy with a grade of 7150.

[0105] In order to more clearly describe the technical solution of the present application, a detailed embodiment is described below as an example.

[0106] Example 1

[0107] The high-ribbed wall panel blank and the mold are sealed by a vacuum bag, and vacuum is drawn to make the high-ribbed wall panel blank bend and deform to contact the mold. The material of the high-ribbed wall panel blank is a high-strength aluminum alloy with a grade of 7150.

[0108] The internal stress distribution of the high-rib wall panel blank after loading is modeled and simulated. Figure 5a~Figure 5c As shown, in order to reduce the difficulty of modeling, a small high-rib wall panel was used for modeling research. Figure 5a~Figure 5bThis is the internal stress distribution cloud diagram of a small high-rib wall panel after loading simulation. It can be seen that there is high stress on the bending ribs of the component, but when the pressure increases first and then decreases, it can be found that the high bending stress will decrease. For example, when loaded to 2.0MPa, see Figure 5a , the maximum bending stress is 486MPa. Figure 5b , when unloaded to 0.3MPa, the maximum bending stress is only 359MPa. Figure 5a and Figure 5b In the figure, the yellow area indicates the area with relatively large stress, and the darker the color, the greater the stress.

[0109] According to the previous analysis, reducing high stress is beneficial to reducing the risk of cracks. Therefore, a new process is proposed to first load the wall panel to 2MPa to cause a large deformation of the component, and then reduce the load to 0.3MPa to reduce the initial stress.

[0110] Furthermore, according to the high temperature and high stress creep rupture relationship in Table 1, when the stress level exceeds 325MPa, the steel will break within 20 minutes at the forming temperature of 170-190℃; while at 160℃, the time before creep rupture can reach 327min and 86min at the stress levels of 300 and 325MPa, which is much longer than the holding time at 170-190℃. Figure 5c At the same time, since the creep forming process is also a stress relaxation process, the stress level on the high ribs will gradually decay, so the creep rupture time will be longer or even no rupture will occur.

[0111] After the small high-ribbed wall panel is first loaded to 2MPa and then reduced to 0.3MPa, the maximum stress level is reduced from 486MPa to 359MPa. Moreover, through simulation, it is found that the maximum initial stress of 359MPa is reduced to below 300MPa after 0.6h. According to Table 1, creep microcracks will not appear in the wall panel within 5h of forming.

[0112] The high-ribbed wall panel blank and the mold connected to the vacuum bag are pushed into the autoclave together, and the pressure and temperature are increased for creep aging treatment to obtain a high-ribbed thin-walled component. After reaching the target pressure and target temperature, the specific time is maintained for 2 to 4 hours to obtain a high-ribbed thin-walled component. Among them, the temperature is increased to 160°C, and the process of increasing the pressure includes: after the pressure is increased to 2MPa, the air pressure is released to 0.3MPa and then maintained at 0.3MPa.

[0113] The high-ribbed thin-walled component obtained in Example 1 is sprayed with a developer. Figure 7 As shown in Figure a. Figure 7 Figure b is Figure 7 In the local enlarged image shown in the rectangular dotted box in Figure a, no cracks are observed.

[0114] Comparative Example 1

[0115] The difference between the comparative example and the embodiment 1 is that after the pressure of the autoclave is increased to 2 MPa, the pressure is kept constant, and the temperature of the autoclave is increased to 160°C and then remains constant. Figure 8 As shown in Figure a. Figure 8 Figure b is Figure 8 In the local enlarged image shown in the rectangular dotted box in Figure a, cracks are observed. Figure 8 The short lines in the ellipse area in Figure b are cracks.

[0116] By comparing the embodiments and comparative examples, it can be seen that the creep aging forming method for high-ribbed thin-walled components will not cause creep microcracks, thereby obtaining high-ribbed thin-walled components with no surface defects and high quality.

[0117] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A creep aging forming method for high-rib thin-walled components, characterized in that: The following steps are involved: The high-rib wall panel blank and the mold are sealed by a vacuum bag, and vacuum is drawn so that the high-rib wall panel blank is bent and deformed to contact the mold, thereby obtaining a wall panel mold sealing structure; According to the first mapping relationship among the creep forming temperature, bending stress and fracture time of the material corresponding to the high-ribbed wall panel blank, the target forming temperature and the corresponding target bending stress are determined; wherein the target forming temperature is selected from the optional forming temperature range of the high-ribbed wall panel blank, and the forming time corresponding to the target forming temperature is less than the fracture time corresponding to the target forming temperature in the first mapping relationship; Simulating the internal stress distribution of the high-ribbed wall panel blank after loading, and determining the second air pressure corresponding to the high-ribbed wall panel blank under the target bending stress; The wall panel mold sealing structure is placed in an autoclave, and the pressure and temperature are increased to perform creep aging treatment to obtain a high-rib thin-walled component; wherein the process of increasing the pressure includes: increasing the pressure to a first pressure, releasing the pressure to a second pressure, and then maintaining the second pressure; the target temperature of the increased temperature is the target forming temperature.

2. The creep aging forming method of high-rib thin-walled components according to claim 1, characterized in that: The step of determining a first mapping relationship among the creep forming temperature, the bending stress and the fracture time comprises: The material corresponding to the high-rib wall panel blank is subjected to a material creep rupture experiment under conditions of different creep forming temperatures and different bending stresses, and a creep forming temperature-bending stress-rupture time relationship diagram is drawn to obtain the first mapping relationship.

3. The creep aging forming method of high-rib thin-walled components according to claim 1, characterized in that: The step of simulating the internal stress distribution of the high-ribbed wall panel blank after loading to determine the second air pressure corresponding to the high-ribbed wall panel blank under the target bending stress includes: Establish a simulation model of internal stress distribution of high-ribbed wall panel blank after loading; An internal stress distribution cloud map is calculated according to the simulation model, and a second air pressure corresponding to the high-rib wall panel blank under the target bending stress is determined based on the internal stress distribution cloud map.

4. The creep aging forming method for high-ribbed thin-walled components according to claim 3, characterized in that: The steps of establishing a simulation model of the internal stress distribution of the high-rib wall panel blank after loading include: The high-ribbed wall panel blank is meshed by finite element units, and material properties are assigned to the high-ribbed wall panel blank. Symmetrical constraints and linear air pressure loading boundary conditions are applied to obtain the simulation model.

5. The creep aging forming method for high-rib thin-walled components according to claim 1, characterized in that: The step of determining the optional forming temperature range comprises: The material constitutive equation of the high-ribbed wall plate blank is fitted until the error between the fitted creep curve and the experimental creep curve is less than 5%, and the fitted constitutive equation is obtained; Based on the fitted constitutive equation, the creep aging forming of the high-rib wall panel blank is simulated to obtain an optional forming temperature range and a corresponding optional forming time.

6. The creep aging forming method for high-rib thin-walled components according to claim 1, characterized in that: The optional forming temperature range is 120-200°C, and the target forming temperature is 155-165°C.

7. The creep aging forming method for high-rib thin-walled components according to claim 1, characterized in that: In the step of increasing the pressure to the first gas pressure, the pressure increasing rate is 20-50 kPa / min; in the step of increasing the temperature, the temperature increasing rate is 1-3°C / min.

8. The creep aging forming method for high-ribbed thin-walled components according to claim 7, characterized in that: The speed of releasing air pressure is 20~50kPa / min.

9. The creep aging forming method for high-ribbed thin-walled components according to claim 7, characterized in that: The first air pressure ranges from 1.5 to 2.0 MPa, and the second air pressure ranges from 0.3 to 0.5 MPa.

10. The creep aging forming method for high-ribbed thin-walled components according to any one of claims 1 to 9, characterized in that: The material of the high-rib wall panel blank is aluminum alloy.

Citation Information

Patent Citations

  • Method for forming large-curvature integral aluminum component

    AU2021100534A4

  • Age hardenable aluminum alloy integral panel one-step forming method based on autoclave

    CN103691793A