Magnesium phosphate cement for tunnel crack repair and preparation method thereof
By adding retarder, temperature control agent and viscosity reducing agent to magnesium phosphate cement, it extends its final settling time and improves interface bonding performance, the strength retraction and aging of existing tunnel concrete crack repair materials has been solved, and the problem of improvement of the strength of the existing tunnel concrete crack repair materials has been improved. Service performance and lifespan of tunnel structures.
Patent Information
- Application Number
- CN202411087790.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The existing tunnel concrete crack repair materials have problems such as difficulty in coagulation and hardening control, later strength reversal, low bond strength, easy aging and high-temperature environment deformation, which has led to a gradual reduction in the service performance of the engineering structure and increased operation and maintenance costs.
Magnesium raw materials, phosphate materials and mineral admixture materials are used as the main components, and retarder, temperature control agent and viscosity reducing agent are added to extend the final settling time of magnesium phosphate cement, improve the slurry flow and interface bonding performance.
The final settling time of magnesium phosphate cement is extended, compressive strength is improved, and interface bonding strength is enhanced, which reduces operation and maintenance costs and extends the service life of the tunnel concrete structure.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of engineering structure repair, and particularly relates to magnesium phosphate cement for tunnel crack repair and a preparation method thereof. Background Art
[0002] As the service life of tunnel engineering structures increases, they will inevitably be affected by the external environment, causing damage such as breakage, cracking, and peeling on the concrete surface, which will cause the performance of the concrete structure to deteriorate, resulting in reduced service safety. In addition, during the service process, the concrete structure may be damaged or destroyed by geological disasters such as earthquakes, storms, floods and other uncontrollable factors, seriously affecting its service performance, causing economic losses and casualties. For these old and damaged concrete structures, the possibility of complete demolition and reconstruction is very small. In order to extend their service life and improve stability and safety, the demand for concrete structure repair and reinforcement is gradually increasing, and the market prospects are broad.
[0003] At present, the commonly used materials for repairing and reinforcing tunnel concrete cracks are sulphoaluminate repair mortars, epoxy resin repair mortars and other repair and reinforcement materials. However, this type of material has the disadvantages of difficult coagulation and hardening control, later strength shrinkage, low bonding strength, high production of finished products, easy deformation in high temperature environment, and easy aging. After repairing and reinforcing the engineering structure, the service safety of the engineering structure will be improved for a certain period of time. However, with the passage of time, the degradation of the performance of traditional repair and reinforcement materials is bound to lead to a further reduction in the safety and stability of the engineering structure, affecting its service performance. However, in order to ensure the safety of the engineering structure, it needs to be repaired and reinforced again. Such a reciprocating cycle leads to a significant increase in costs during the operation and maintenance of the engineering structure.
[0004] Magnesium phosphate cement is a material with very significant individuality. It has the characteristics of rapid setting and hardening, excellent hourly strength, high bonding strength with concrete interface, small shrinkage, high temperature resistance, and excellent frost resistance. It has broad application prospects in the repair and reinforcement of damaged concrete structures. However, magnesium phosphate cement has a short setting time and relatively poor construction performance, which greatly limits the promotion and application of magnesium phosphate cement in multiple scenarios. Therefore, extending its setting time and further improving its working performance through effective control measures is the key to achieving the promotion and application of magnesium phosphate cement. The achievement of this goal can solve the problems of low bonding performance, easy aging, and later strength shrinkage of existing repair and reinforcement materials, which is of great significance to the improvement of the service performance of tunnel lining concrete structures. Summary of the invention
[0005] The object of the present invention is to provide a magnesium phosphate cement for tunnel crack repair and a preparation method thereof in accordance with the above-mentioned deficiencies of the prior art. The magnesium phosphate cement is prepared by taking magnesium raw materials, phosphate materials and mineral admixtures as main components, and adding retarders, temperature control agents and viscosity reducers thereto, thereby extending the final setting time of the magnesium phosphate cement, improving the fluidity of the slurry, and improving the hourly strength and interface bonding performance.
[0006] The purpose of the present invention is achieved by the following technical solutions:
[0007] A magnesium phosphate cement for tunnel crack repair, comprising the following mass components: 50%-70% magnesium raw material, 20%-30% phosphate material, 10%-20% mineral admixture, the sum of the three being 100%;
[0008] In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: retarder 2%-8%, temperature control agent 4%-12%, and viscosity reducer 2%-10%.
[0009] The magnesium raw material is one or a combination of periclase, serpentine and talc; the content of MgO in the chemical composition of the magnesium raw material is greater than 30%.
[0010] The phosphate material is one or a combination of two of potassium hypophosphite, disodium dihydrogen pyrophosphate, and sodium aluminum acid phosphate.
[0011] The mineral admixture is one or a combination of two of circulating fluidized bed fly ash, silica ash and bentonite.
[0012] The retarder is one or a combination of two of diaminophosphate, trimethyl myristyl ammonium chloride, and trimethyl ammonium chloride; the temperature control agent is one or a combination of two of microcrystalline paraffin, triisopropyl borate, and sodium tetrapropyl borate; the viscosity reducer is one or two of polyethylene ether ethyl ether, polyethylene ether ester, and hexadecyl polyoxyethylene ether.
[0013] The magnesium phosphate cement comprises the following mass components: 50% magnesium raw material, 30% phosphate material, and 20% mineral admixture, the sum of which is 100%; wherein the magnesium raw material is talc, the content of MgO in the talc is 56.2%, the phosphate material is sodium aluminum acid phosphate, and the mineral admixture is circulating fluidized bed fly ash;
[0014] In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: 8% retarder, 12% temperature control agent, and 10% viscosity reducer; wherein the retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
[0015] The magnesium phosphate cement comprises the following mass components: 60% magnesium raw material, 26% phosphate material, and 14% mineral admixture, the sum of which is 100%; wherein the magnesium raw material is talc, the content of MgO in the talc is 50.5%, the phosphate material is sodium aluminum acid phosphate, and the mineral admixture is circulating fluidized bed fly ash;
[0016] In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: 6% retarder, 9% temperature control agent, and 8% viscosity reducer; wherein the retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
[0017] The magnesium phosphate cement comprises the following mass components: 65% magnesium raw material, 23% phosphate material, and 12% mineral admixture, the sum of which is 100%; wherein the magnesium raw material is talc, the content of MgO in the talc is 45.7%, the phosphate material is sodium aluminum acid phosphate, and the mineral admixture is circulating fluidized bed fly ash;
[0018] In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: 4% retarder, 6% temperature control agent, and 5% viscosity reducer; wherein the retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
[0019] The magnesium phosphate cement comprises the following mass components: 70% magnesium raw material, 20% phosphate material, and 10% mineral admixture, the sum of which is 100%; wherein the magnesium raw material is talc, the content of MgO in the talc is 40.6%, the phosphate material is sodium aluminum acid phosphate, and the mineral admixture is circulating fluidized bed fly ash;
[0020] In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: 2% retarder, 4% temperature control agent, and 2% viscosity reducer; wherein the retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
[0021] A method for preparing any of the magnesium phosphate cements for tunnel crack repair, the method comprising the following steps:
[0022] S1: Grind the magnesium raw material and mineral admixture in a ball mill to control the surface area of the obtained powder to 300m 2 / kg-500m 2 / kg;
[0023] S2: placing the powder obtained in step S1 in a mixer, then adding phosphate materials and mixing for 30 minutes; finally, additional functional regulating components are added, and the order of adding the components in the functional regulating components is: first adding a retarder and stirring for 10 minutes, then adding a temperature control agent and stirring for 10 minutes, and finally adding a viscosity reducer and continuing to stir for 20 minutes to obtain magnesium phosphate cement.
[0024] The invention has the advantages that: it is proposed to use magnesium phosphate cement as a repair and reinforcement material for tunnel lining concrete cracks. Under the synergistic effect of a retarder, a temperature control agent and a viscosity reducer, the final setting time of the obtained magnesium phosphate cement repair and reinforcement material can be controlled at about 1.5 hours, the slurry fluidity can be controlled at about 280 mm, the 2h compressive strength can reach about 30 MPa, the 1d compressive strength can reach about 45 MPa, the 28d compressive strength can reach about 70 MPa, the interface pull-out bond strength with the concrete matrix at 2h can reach about 0.9 MPa, the 1d interface pull-out bond strength is about 1.7 MPa, and the 28d interface pull-out bond strength is higher than the tensile strength of the concrete matrix. The concrete matrix is damaged during the stretching process, and the interface bonding between the magnesium phosphate cement and the concrete is not damaged. The magnesium phosphate cement prepared by the technology of the invention can completely replace the existing repair and reinforcement material as a repair and reinforcement treatment for damaged concrete structures, reduce the operation and maintenance cost during its service, and effectively improve its service life. DETAILED DESCRIPTION
[0025] The features of the present invention and other related features are further described in detail below through embodiments to facilitate understanding by those skilled in the art:
[0026] A magnesium phosphate cement for tunnel crack repair and a preparation method thereof, comprising the following mass components: 50%-70% magnesium raw material, 20%-30% phosphate material, 10%-20% mineral admixture, the sum of the three being 100%; in addition, the magnesium phosphate cement also comprises an additional functional regulating component, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, comprises: 2%-8% retarder, 4%-12% temperature control agent, and 2%-10% viscosity reducer. Among them:
[0027] The magnesium raw material is talc, and the content of MgO in the chemical composition of talc is 40.6%-56.2%. The phosphate material is sodium aluminum acid phosphate. The mineral admixture is circulating fluidized bed fly ash, which is produced by the combustion of a circulating fluidized bed boiler.
[0028] The retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
[0029] Based on the above mass component range of magnesium phosphate cement, 4 example formulas are provided, and 5 comparative examples are provided to test and compare the final setting time, fluidity, tensile bond strength and compressive strength of magnesium phosphate cement in different component intervals and outside the component range.
[0030] Example 1: This example specifically relates to a magnesium phosphate cement for tunnel crack repair, wherein the main components of the magnesium phosphate cement include the following mass components: 50% talc, 30% sodium aluminum acid phosphate, and 20% circulating fluidized bed fly ash, the sum of which is 100%; wherein the MgO content in the talc used is 56.2%.
[0031] In addition, functional regulating components are additionally added to magnesium phosphate cement, and the functional regulating components include (in terms of the mass percentage of magnesium raw material talc and mineral admixture circulating fluidized bed fly ash): 8% trimethylammonium chloride, 12% microcrystalline wax, and 10% hexadecyl polyoxyethylene ether. It should be noted that the functional regulating components here are additionally added to the main components on the basis that the sum of the mass percentages of the main components is 100%, and the mass percentage of each component in the functional regulating components is the mass percentage when compared with the mass of magnesium raw material talc and mineral admixture circulating fluidized bed fly ash.
[0032] The preparation method of the magnesium phosphate cement for tunnel crack repair in this embodiment comprises the following steps:
[0033] (S1) Raw material grinding: 5 kg of talc and circulating fluidized bed fly ash were weighed accurately according to the mass percentage of the main components and ground in a ball mill to control the surface area of the obtained powder to 300 m 2 / kg-350m 2 / kg.
[0034] (S2) Mixing: The powder obtained in step ① is placed in a mixer, and the phosphate material sodium aluminum phosphate is first added according to the mass percentage, and the mixture is stirred for 30 minutes; then, based on the mass of the magnesium raw material talc and the mineral admixture circulating fluidized bed fly ash in the main components being 100%, additional functional regulating components are added in the following order: first, a retarder trimethylammonium chloride is added and stirred for 10 minutes, then a temperature control agent microcrystalline paraffin is added and stirred for 10 minutes, and finally, a viscosity reducer hexadecyl polyoxyethylene ether is added and stirred for 20 minutes to obtain the magnesium phosphate cement.
[0035] Example 2: This example specifically relates to a magnesium phosphate cement for tunnel crack repair, the main components of which include the following mass components: 60% talc, 26% sodium aluminum acid phosphate, and 14% circulating fluidized bed fly ash, the sum of which is 100%. The talc used in this example has a MgO content of 50.5%.
[0036] In addition, a functional regulating component is additionally added to the magnesium phosphate cement, and the functional regulating component includes (in terms of the mass percentage of the magnesium raw material talc and the circulating fluidized bed fly ash of the mineral admixture): 6% trimethylammonium chloride, 9% microcrystalline wax, and 8% hexadecyl polyoxyethylene ether. It should be noted that the functional regulating component here is additionally added to the main component on the basis that the sum of the mass percentages of the main components is 100%, and the mass percentage of each component in the functional regulating component is the mass percentage when compared with the mass of the magnesium raw material talc and the circulating fluidized bed fly ash of the mineral admixture.
[0037] The preparation method of the magnesium phosphate cement for tunnel crack repair in this embodiment comprises the following steps:
[0038] (S1) Raw material grinding: 5 kg of talc and circulating fluidized bed fly ash were weighed accurately according to the mass percentage of the main components and ground in a ball mill to control the surface area of the obtained powder to 350 m 2 / kg-400m 2 / kg.
[0039] (S2) Mixing: The powder obtained in step ① is placed in a mixer, and the phosphate material sodium aluminum phosphate is first added according to the mass percentage, and the mixture is stirred for 30 minutes; then, based on the mass of the magnesium raw material talc and the mineral admixture circulating fluidized bed fly ash in the main components being 100%, additional functional regulating components are added in the following order: first, a retarder trimethylammonium chloride is added and stirred for 10 minutes, then a temperature control agent microcrystalline paraffin is added and stirred for 10 minutes, and finally, a viscosity reducer hexadecyl polyoxyethylene ether is added and stirred for 20 minutes to obtain the magnesium phosphate cement.
[0040] Example 3: This example specifically relates to a magnesium phosphate cement for tunnel crack repair, the main components of which include the following mass components: 65% talc, 23% sodium aluminum acid phosphate, and 12% circulating fluidized bed fly ash, the sum of which is 100%. The talc used in this example has a MgO content of 45.7%.
[0041] In addition, a functional regulating component is additionally added to the magnesium phosphate cement, and the functional regulating component includes (in terms of the mass percentage of the magnesium raw material talc and the circulating fluidized bed fly ash of the mineral admixture): 4% trimethylammonium chloride, 6% microcrystalline wax, and 5% hexadecyl polyoxyethylene ether. It should be noted that the functional regulating component here is additionally added to the main component on the basis that the sum of the mass percentages of the main components is 100%, and the mass percentage of each component in the functional regulating component is the mass percentage when compared with the mass of the magnesium raw material talc and the circulating fluidized bed fly ash of the mineral admixture.
[0042] The preparation method of the magnesium phosphate cement for tunnel crack repair in this embodiment comprises the following steps:
[0043] (S1) Raw material grinding: 5 kg of talc and circulating fluidized bed fly ash were weighed accurately according to the mass percentage of the main components and ground in a ball mill to control the surface area of the obtained powder to 400 m 2 / kg-450m 2 / kg.
[0044] (S2) Mixing: The powder obtained in step ① is placed in a mixer, and the phosphate material sodium aluminum phosphate is first added according to the mass percentage, and the mixture is stirred for 30 minutes; then, based on the mass of the magnesium raw material talc and the mineral admixture circulating fluidized bed fly ash in the main components being 100%, additional functional regulating components are added in the following order: first, a retarder trimethylammonium chloride is added and stirred for 10 minutes, then a temperature control agent microcrystalline paraffin is added and stirred for 10 minutes, and finally, a viscosity reducer hexadecyl polyoxyethylene ether is added and stirred for 20 minutes to obtain the magnesium phosphate cement.
[0045] Example 4: This example specifically relates to a magnesium phosphate cement for tunnel crack repair, wherein the main components of the magnesium phosphate cement include the following mass components: talc 70%, sodium aluminum acid phosphate 20%, circulating fluidized bed fly ash 10%, and the sum of the three is 100%. The talc used in this example has a MgO content of 40.6%.
[0046] In addition, a functional regulating component is additionally added to the magnesium phosphate cement, and the functional regulating component includes (in terms of the mass percentage of the magnesium raw material talc and the circulating fluidized bed fly ash of the mineral admixture): 2% trimethylammonium chloride, 4% microcrystalline wax, and 2% hexadecyl polyoxyethylene ether. It should be noted that the functional regulating component here is additionally added to the main component on the basis that the sum of the mass percentages of the main components is 100%, and the mass percentage of each component in the functional regulating component is the mass percentage when compared with the mass of the magnesium raw material talc and the circulating fluidized bed fly ash of the mineral admixture.
[0047] Comparative Example 1: In this comparative example, no retarder trimethylammonium chloride is added, and the rest is the same as Example 1.
[0048] Comparative Example 2: In this comparative example, the temperature control agent microcrystalline paraffin is not added, and the rest is the same as Example 2.
[0049] Comparative Example 3: In this comparative example, the viscosity reducing agent hexadecyl polyoxyethylene ether was not added, and the rest was the same as Example 3.
[0050] Comparative Example 4: In this comparative example, no function regulating component is added, and the rest is the same as Example 1.
[0051] Comparative Example 5: In this comparative example, the magnesium raw material talc is completely replaced by heavy-burned magnesium oxide, a magnesium raw material commonly used in preparing magnesium phosphate cement, and the phosphate material sodium aluminum acid phosphate is completely replaced by potassium dihydrogen phosphate, a commonly used phosphate for preparing magnesium phosphate cement, and the rest is the same as Example 1.
[0052] After the above-mentioned embodiments and comparative examples were mixed with water at a water-cement ratio of 0.45, the setting time of each embodiment and comparative example was tested according to GB / T1346-2019 "Test Method for Standard Consistency, Setting Time and Stability of Cement"; the fluidity of each embodiment and comparative example was tested according to GB / T 8077-2012 "Test Method for Homogeneity of Concrete Admixtures"; the compressive strength and interfacial tensile bond strength of each embodiment and comparative example at 2h, 1d and 28d were tested according to GB / T 17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)" and JGJ / T70-2009 "Standard for Test Method for Basic Performance of Building Mortar". The test results of each embodiment and comparative example are shown in Table 1.
[0053] Table 1 Performance indicators of magnesium phosphate cement
[0054] .
[0055] Note: When testing the interface tensile strength, the matrix concrete used is C50, and the tensile strength of the concrete matrix itself is 2.6MPa. The “—” in the table means that when testing the tensile bond strength of the interface between magnesium phosphate cement and concrete matrix, the damage occurs inside the concrete matrix, that is, the tensile bond strength of the interface between magnesium phosphate cement and concrete matrix is greater than 2.6MPa.
[0056] It can be seen from the results in Table 1 that the setting time of magnesium phosphate cement in Examples 1-4 can be controlled to be more than 1h, and the fluidity of the slurry is greater than 260mm. In terms of interfacial tensile bond strength, the interfacial tensile bond strength of the magnesium phosphate cement prepared by the present invention can reach 0.6MPa and 1.4MPa or more at 2h and 1d, respectively. At 28d, its interfacial tensile bond strength with the concrete matrix is higher than the tensile strength of the concrete matrix, and the damage occurs inside the concrete, indicating that the tensile bond strength of the magnesium phosphate cement prepared by the present invention with the concrete matrix is very excellent. In terms of compressive strength, the compressive strength of the magnesium phosphate cement prepared by the present invention at 2h and 1d is greater than 26.1MPa and 40.6MPa, respectively, and the 28d compressive strength is more than 67MPa, and the strength development is good. This technical invention realizes the effective extension of the setting time of magnesium phosphate cement and the significant improvement of working performance, and takes into account the coordinated development of its mechanical properties, and the implementation effect is remarkable.
[0057] Compared with Example 1, the lack of retarder in the functional control component in Comparative Example 1 significantly shortens the setting time of magnesium phosphate cement, but has little effect on the fluidity of the slurry. At the same time, due to the lack of retarder, the reaction rate is too fast, and the generated reaction products are wrapped on the surface of the unreacted particles, resulting in a decrease in the reaction degree of magnesium phosphate cement, which in turn causes the compressive strength of magnesium phosphate cement and the tensile bond strength of the interface with concrete to decrease to varying degrees.
[0058] Compared with Example 2, due to the lack of a temperature control agent in the functional control component, the temperature of the magnesium phosphate cement system in Comparative Example 2 rises too fast during the reaction, and the reaction rate increases, which causes its setting time and slurry fluidity to decrease significantly. At the same time, due to the excessively fast reaction rate, the wrapping effect of the reaction product also causes the reaction degree of the magnesium phosphate cement to decrease, resulting in a decrease in its compressive strength and the tensile bond strength of the interface with the concrete.
[0059] Compared with Example 3, due to the lack of viscosity reducer in the functional control component, the slurry viscosity of Comparative Example 3 is too high, resulting in a significant decrease in the fluidity of magnesium phosphate cement. Due to the high slurry viscosity, magnesium phosphate cement is difficult to penetrate into the concrete matrix, resulting in a significant decrease in the tensile bond strength of the interface with the concrete. At the same time, a certain amount of gas is introduced during the stirring process of magnesium phosphate cement, and excessive viscosity will cause this part of the gas to be unable to be released, resulting in an increase in the porosity of the hardened matrix, which in turn leads to a decrease in the compressive strength of the matrix.
[0060] Compared with Example 1, due to the lack of functional regulating components, the reaction rate of the magnesium phosphate cement obtained in Comparative Example 4 is high, the temperature rise of the system is accelerated, and the slurry viscosity is also high. Under the combined effect of the above factors, the setting time of the magnesium phosphate cement is significantly shortened to only 12 minutes, and the flow of the slurry and the mechanical properties of the hardened slurry are also significantly reduced.
[0061] Compared with Example 1, in Comparative Example 5, the magnesium raw material talc is completely replaced by the commonly used magnesium raw material dead-burned magnesium oxide for preparing magnesium phosphate cement, and the phosphate material sodium aluminum acid phosphate is completely replaced by the commonly used phosphate potassium dihydrogen phosphate for preparing magnesium phosphate cement. The setting time of the obtained magnesium phosphate cement is slightly shortened, and the slurry fluidity and the compressive strength of the magnesium phosphate cement and the tensile bonding strength of the interface with the concrete are not greatly reduced. This result also shows that the functional control component described in the present invention is also suitable for the control of the setting and hardening properties, working properties and mechanical properties of magnesium phosphate cement currently prepared using dead-burned magnesium oxide and potassium dihydrogen phosphate as raw materials.
[0062] The above embodiments are only used to explain the present invention and do not constitute a limitation on the scope of the claims. Other alternative means that can be thought of by those skilled in the art based on the contents of the present specification should be within the protection scope of the claims of the present invention.
Claims
1. A magnesium phosphate cement for tunnel crack repair, characterized in that The magnesium phosphate cement comprises the following mass components: 50%-70% magnesium raw material, 20%-30% phosphate material, 10%-20% mineral admixture, the sum of the three being 100%; In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: 2%-8% retarder, 4%-12% temperature control agent, and 2%-10% viscosity reducer; The magnesium raw material is talc, the phosphate material is sodium aluminum acid phosphate, and the mineral admixture is circulating fluidized bed fly ash; The retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
2. The magnesium phosphate cement for tunnel crack repair according to claim 1, characterized in that The magnesium phosphate cement comprises the following mass components: 50% magnesium raw material, 30% phosphate material, and 20% mineral admixture, the sum of which is 100%; wherein the magnesium raw material is talc, the content of MgO in the talc is 56.2%, the phosphate material is sodium aluminum acid phosphate, and the mineral admixture is circulating fluidized bed fly ash; In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: 8% retarder, 12% temperature control agent, and 10% viscosity reducer; wherein the retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
3. The magnesium phosphate cement for tunnel crack repair according to claim 1, characterized in that The magnesium phosphate cement comprises the following mass components: 60% magnesium raw material, 26% phosphate material, and 14% mineral admixture, the sum of which is 100%; wherein the magnesium raw material is talc, the content of MgO in the talc is 50.5%, the phosphate material is sodium aluminum acid phosphate, and the mineral admixture is circulating fluidized bed fly ash; In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: 6% retarder, 9% temperature control agent, and 8% viscosity reducer; wherein the retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
4. The magnesium phosphate cement for tunnel crack repair according to claim 1, characterized in that The magnesium phosphate cement comprises the following mass components: 65% magnesium raw material, 23% phosphate material, and 12% mineral admixture, the sum of which is 100%; wherein the magnesium raw material is talc, the content of MgO in the talc is 45.7%, the phosphate material is sodium aluminum acid phosphate, and the mineral admixture is circulating fluidized bed fly ash; In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: 4% retarder, 6% temperature control agent, and 5% viscosity reducer; wherein the retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
5. The magnesium phosphate cement for tunnel crack repair according to claim 1, characterized in that The magnesium phosphate cement comprises the following mass components: 70% magnesium raw material, 20% phosphate material, and 10% mineral admixture, the sum of which is 100%; wherein the magnesium raw material is talc, the content of MgO in the talc is 40.6%, the phosphate material is sodium aluminum acid phosphate, and the mineral admixture is circulating fluidized bed fly ash; In addition, the magnesium phosphate cement also includes additional functional regulating components, which, in terms of the mass percentage of the magnesium raw material and the mineral admixture, include: 2% retarder, 4% temperature control agent, and 2% viscosity reducer; wherein the retarder is trimethylammonium chloride, the temperature control agent is microcrystalline paraffin, and the viscosity reducer is hexadecyl polyoxyethylene ether.
6. A method for preparing magnesium phosphate cement for tunnel crack repair according to any one of claims 1 to 5, characterized in that The preparation method comprises the following steps: S1: Grind the magnesium raw material and the mineral admixture in a ball mill to control the surface area of the obtained powder to be 300m2 / kg-500m2 / kg; S2: placing the powder obtained in step S1 in a mixer, then adding phosphate materials and mixing for 30 minutes; finally, additional functional regulating components are added, and the order of adding the components in the functional regulating components is: first adding a retarder and stirring for 10 minutes, then adding a temperature control agent and stirring for 10 minutes, and finally adding a viscosity reducer and continuing to stir for 20 minutes to obtain magnesium phosphate cement.