A preparation method of a large-pore self-healing porous medium burn-out hole-forming rotating tube and a rotating tube

Through the modification of expanded graphite slurry and two sintering technology, the skeleton structure is formed and the gap in the rotating tube is healed, which solves the problem of void after the porous sponge body is limited, and the thermal shock resistance and service life of the glass rotating tube is significantly improved.

CN118598648BActive Publication Date: 2024-12-06HUNAN KIBING PHARMACEUTICAL MATERIAL TECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410846778.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-12-06
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

The porous sponge used in the existing glass drawing process has a millimeter-level gap behind the limiting parts, resulting in stress concentration and crack expansion, and poor thermal vibration resistance.

Method used

The porous sponge is treated with modified expanded graphite slurry, and the frame structure is formed through two sintering to avoid the skeleton collapse and heal the large internal gap. Organic limiting parts are used to maintain the position of the sponge body, and the limiting parts disappear after sintering.

Benefits of technology

It effectively eliminates millimeter-level gaps, improves the thermal shock resistance of the rotating tube, can resist multiple thermal shock cycles, and extends the service life.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of glass production equipment, and in particular to a preparation method and a rotating tube for a large-pore self-healing porous medium burn-out hole-forming rotating tube, comprising the following steps: dissolving Al powder, C powder, SIC powder and expanded graphite in deionized water, stirring and filtering, and drying the filtered product and sintering it in a nitrogen atmosphere, and grinding it into powder after sintering; soaking a porous sponge in a modified expanded graphite slurry, and then drying the porous sponge containing the modified expanded graphite slurry in the shade; placing the porous sponge containing the modified expanded graphite slurry after the shade drying into the inner liner of a rotating tube mold, injecting the rotating tube slurry into the inner liner of the rotating tube mold, and demolding after the shade drying to form a semi-finished product; sintering for the first time until the porous sponge is completely decomposed; after the first sintering is completed, sintering for the second time until the large gaps in the rotating tube are healed. This scheme effectively heals large gaps and improves thermal shock resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass production equipment, in particular to a preparation method of a macroporous self-healing porous medium burn-out pore-forming rotating tube and a rotating tube. Background Art

[0002] A rotating tube is required in the glass drawing process. A Chinese patent with application number CN202310569554.2 discloses a 3D printed porous medium burn-out hole-forming rotating tube preparation process and mold. The rotating tube is prepared by the porous medium burn-out hole-forming method, and a special mold is used to cooperate with the firing of the rotating tube, which improves the thermal shock resistance and significantly reduces the weight.

[0003] However, the above method uses a limiter to limit the porous sponge body, thereby effectively controlling the position of the porous sponge body. However, after the limiter is burned out, there are millimeter-level gaps in the original position of the limiter, which are prone to stress concentration, leading to crack expansion and poor thermal vibration resistance. Summary of the invention

[0004] The present invention provides a method for preparing a macroporous self-healing porous medium burn-out hole-forming rotating tube and a rotating tube, so as to solve the problem that after the porous sponge body is limited in the prior art, there is a millimeter-level gap in the original position of the limiter.

[0005] In order to alleviate the above technical problems, the technical solution provided by the present invention is:

[0006] A method for preparing a macroporous self-healing porous medium burn-out hole-forming rotating tube comprises the following steps:

[0007] 1) preparing modified expanded graphite slurry: dissolving Al powder, C powder, SIC powder and expanded graphite in deionized water, stirring and filtering, drying the filtered product and sintering it in a nitrogen atmosphere, grinding it into powder after sintering, and then dissolving the powdered modified expanded graphite in water to form a modified expanded graphite slurry;

[0008] 2) soaking the porous sponge in modified expanded graphite slurry, and then drying the porous sponge containing the modified expanded graphite slurry in the shade;

[0009] 3) placing the air-dried porous sponge containing the modified expanded graphite slurry into the inner liner of a rotating tube mold, injecting the rotating tube slurry into the inner liner of the rotating tube mold, and demoulding after air-drying to form a semi-finished product;

[0010] 4) First sintering until the porous sponge is completely decomposed;

[0011] 5) After the first sintering is completed, the second sintering is carried out until the large gaps in the rotating tube are healed.

[0012] Furthermore,

[0013] In the step of preparing the modified expanded graphite slurry, the weight ratio of Al powder: C powder: SIC powder: expanded graphite is (1-3): (4-6): (1-3): (40-50).

[0014] Furthermore,

[0015] In the step of preparing the modified expanded graphite slurry, the weight ratio of Al powder: C powder: SIC powder: expanded graphite is 2:5:2:45.

[0016] Furthermore,

[0017] In the step of preparing the modified expanded graphite slurry, the filtered product is dried and then sintered in a nitrogen atmosphere under high pressure.

[0018] Furthermore,

[0019] The first sintering temperature is 1200-1500 degrees Celsius.

[0020] Furthermore,

[0021] The second sintering temperature is 800-1000 degrees Celsius.

[0022] Furthermore,

[0023] The rotary tube slurry includes the following raw materials in parts by weight:

[0024] 50-70 parts of high-purity sintered mullite;

[0025] 8-20 parts of talc;

[0026] 7-15 parts of aluminum oxide powder;

[0027] 4-10 parts of silica powder;

[0028] 3-25 parts of binding clay;

[0029] 5 to 10 parts of modified expanded graphite slurry.

[0030] Furthermore,

[0031] The porous sponge body is immersed in the modified expanded graphite slurry through a limiting piece to keep the position of the porous sponge body in the slurry from being offset.

[0032] Furthermore,

[0033] The limiting member is made of an organic material, and the limiting member disappears after sintering.

[0034] A rotating tube is prepared by the above-mentioned method for preparing a rotating tube with large pores and self-healing porous media through burning out.

[0035] The effect analysis is as follows:

[0036] Expanded Graphite is a carbonaceous raw material obtained by chemically or electrochemically intercalating natural flake graphite and then instantaneously heating it to produce high-temperature expansion.

[0037] Expanded graphite has many excellent properties. It not only retains many advantages of natural graphite, such as high temperature resistance, electrical conductivity, thermal conductivity, lubricity, special thermal shock resistance, chemical stability and corrosion resistance, but also has the characteristics of developed pore structure, high reactivity, large specific surface area, high compression rate and high elasticity that natural graphite does not have. However, expanded graphite is prone to collapse and agglomeration.

[0038] This scheme uses Al powder, C powder, and SIC powder to modify expanded graphite in a nitrogen atmosphere to obtain modified expanded graphite, forming ceramic whiskers such as AlN, Al4C3 and SiC. The ceramic whiskers and expanded graphite are synergistically toughened. After a large number of voids are formed after the porous sponge is sintered for the first time, the modified expanded graphite forms a skeleton structure. Since the expanded graphite is modified, the collapse of the skeleton structure is effectively avoided.

[0039] Research has found that after the first sintering, the porous sponge inside disappears; after the second sintering, the modified expanded graphite expands linearly and migrates, filling the large gap in the rotating tube until it heals.

[0040] In addition, after the skeleton structure formed by modified expanded graphite is formed inside the rotating tube, the heat transfer path of the rotating tube is interrupted, which can effectively prevent external heat energy from being transferred to the main shaft of the rotating tube, thereby increasing the service life of the main shaft of the rotating tube. DETAILED DESCRIPTION

[0041] Example 1

[0042] This embodiment provides a method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube, comprising the following steps:

[0043] 1) Prepare modified expanded graphite slurry: dissolve Al powder, C powder, SIC powder and expanded graphite in deionized water, stir and filter, wherein the weight ratio of Al powder: C powder: SIC powder: expanded graphite is 2:5:2:45. Dry the filtered product and sinter it in a nitrogen atmosphere, grind it into powder after sintering, and then dissolve the powdered modified expanded graphite in water to form a modified expanded graphite slurry;

[0044] 2) soaking the porous sponge in modified expanded graphite slurry, and then drying the porous sponge containing the modified expanded graphite slurry in the shade;

[0045] 8.3) placing the air-dried porous sponge containing the modified expanded graphite slurry into the inner liner of a rotating tube mold, injecting the rotating tube slurry into the inner liner of the rotating tube mold, air-drying to form a semi-finished product and then demolding; the rotating tube slurry comprises the following raw materials in parts by weight: 50-70 parts of high-purity sintered mullite; 8-20 parts of talc; 7-15 parts of alumina powder; 4-10 parts of silica powder; 3-25 parts of binding clay; and 5-10 parts of modified expanded graphite slurry.

[0046] 4) The first sintering is performed until the porous sponge is completely decomposed, and the sintering temperature is 1300 degrees Celsius.

[0047] 5) After the first sintering is completed, the second sintering is performed until the large gap in the rotating tube is healed. The sintering temperature is 1000 degrees Celsius.

[0048] The cross-section of the corresponding limiter of the sample was observed and the millimeter-level void content was tested, and no millimeter-level voids were found.

[0049] The samples were tested for thermal shock resistance, and the rotating tube prepared by the above process could withstand 48 thermal shock cycles.

[0050] Comparative Example 1

[0051] This example provides a method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube, in which the weight ratio of Al powder: C powder: SIC powder: expanded graphite is 0:7:2:45. The remaining steps are the same.

[0052] The cross-section of the corresponding limiter of the sample was observed and the millimeter-level void content was detected, and a small amount of millimeter-level voids were found.

[0053] The samples were tested for thermal shock resistance, and the rotating tube prepared by the above process could withstand 40 thermal shock cycles.

[0054] Comparative Example 2

[0055] This embodiment provides a method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube, in which the weight ratio of Al powder: C powder: SIC powder: expanded graphite in Embodiment 2 is 2:0:7:45. The remaining steps are the same.

[0056] The cross-section of the corresponding limiter of the sample was observed and the millimeter-level void content was detected, and a small amount of millimeter-level voids were found.

[0057] The samples were tested for thermal shock resistance, and the rotating tube prepared by the above process could withstand 42 thermal shock cycles.

[0058] Comparative Example 3

[0059] This embodiment provides a method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube, and in Example 2, the weight ratio of Al powder: C powder: SIC powder: expanded graphite is 2:7:0:45. The remaining steps are the same.

[0060] The cross-section of the corresponding limiter of the sample was observed and the millimeter-level void content was detected, and a small amount of millimeter-level voids were found.

[0061] The samples were tested for thermal shock resistance, and the rotating tube prepared by the above process could withstand 38 thermal shock cycles.

[0062] Comparative Example 4

[0063] The porous sponge is soaked in expanded graphite slurry (unmodified), and then the porous sponge containing expanded graphite slurry is dried in the shade; the porous sponge containing modified expanded graphite slurry after drying in the shade is placed in the inner liner of the rotating tube mold, and the rotating tube slurry is injected into the inner liner of the rotating tube mold, and the semi-finished product is formed after drying in the shade and then demolded; the first sintering is performed until the porous sponge is completely decomposed, and the sintering temperature is 1300 degrees Celsius. After the first sintering is completed, the second sintering is performed until the large gap in the rotating tube is healed, and the sintering temperature is 1300 degrees Celsius. .

[0064] The cross section of the corresponding stopper of the sample was observed and the millimeter-level void content was detected, and a large number of millimeter-level voids were found. A large number of millimeter-level voids are most likely caused by the agglomeration and collapse of the expanded graphite slurry.

[0065] The samples were tested for thermal shock resistance, and the rotating tube prepared by the above process could withstand 28 thermal shock cycles.

[0066] Comparative Example 5

[0067] In this embodiment, the rotating tube is prepared by the preparation method of application number CN202310569554.2, which can withstand 30 thermal shock cycles.

[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a large-pore self-healing porous medium burn-out pore-forming rotating tube, characterized in that: The steps include: 1) preparing modified expanded graphite slurry: dissolving Al powder, C powder, SIC powder and expanded graphite in deionized water, stirring and filtering, drying the filtered product and sintering it in a nitrogen atmosphere, grinding it into powder after sintering, and then dissolving the powdered modified expanded graphite in water to form modified expanded graphite slurry; the weight ratio of Al powder: C powder: SIC powder: expanded graphite is (1-3): (4-6): (1-3): (40-50); 2) soaking the porous sponge in modified expanded graphite slurry, and then drying the porous sponge containing the modified expanded graphite slurry in the shade; 3) placing the air-dried porous sponge containing the modified expanded graphite slurry into the inner liner of a rotating tube mold, injecting the rotating tube slurry into the inner liner of the rotating tube mold, and demoulding after air-drying to form a semi-finished product; 4) First sintering until the porous sponge is completely decomposed; 5) After the first sintering is completed, the second sintering is carried out until the large gaps in the rotating tube are healed.

2. The method for preparing the macroporous self-healing porous medium burn-out pore-forming rotating tube according to claim 1, characterized in that: In the step of preparing the modified expanded graphite slurry, the weight ratio of Al powder: C powder: SIC powder: expanded graphite is 2:5:2:

45.

3. The method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube according to claim 1, characterized in that: In the step of preparing the modified expanded graphite slurry, the filtered product is dried and then sintered in a nitrogen atmosphere under high pressure.

4. The method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube according to claim 1, characterized in that: The first sintering temperature is 1200-1500 degrees Celsius.

5. The method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube according to claim 1, characterized in that: The second sintering temperature is 800-1000 degrees Celsius.

6. The method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube according to claim 1, characterized in that: The rotary tube slurry includes the following raw materials in parts by weight: 50-70 parts of high-purity sintered mullite; 8-20 parts of talc; 7-15 parts of aluminum oxide powder; 4-10 parts of silica powder; 3-25 parts of binding clay; 5 to 10 parts of modified expanded graphite slurry.

7. The method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube according to claim 1, characterized in that: The porous sponge body is immersed in the modified expanded graphite slurry through a limiting piece to keep the position of the porous sponge body in the slurry from being offset.

8. The method for preparing a macroporous self-healing porous medium burn-out pore-forming rotating tube according to claim 7, characterized in that: The limiting member is made of an organic material, and the limiting member disappears after sintering.

9. A rotating tube, characterized in that: The invention is prepared by the method for preparing the macroporous self-healing porous medium burn-out pore-forming rotary tube according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Preparation method of porous ceramic

    CN105859319A

  • Silicon carbide-graphite riser tube and preparation method thereof

    CN107140996A

  • 3D printing glass rotating tube as well as preparation method and application thereof

    CN115838285A

  • 3D printing porous medium ignition loss pore-forming rotary tube preparation process and mold

    CN117024172A

  • Method of producing LF-ladle magnesia-carbon brick

    JP2022060911A