A kind of nylon 12T and its preparation method and application
Through high-pressure prepolymerization-low-pressure polymerization-atmospheric insulation-solid-phase polycondensation process and the addition of calcium carbonate nucleating agents of different particle sizes, the mechanical properties of nylon 12T are improved, and the problem of insufficient performance of nylon 12T in the existing process is solved. It is suitable for High-performance material requirements for wind power blades.
Patent Information
- Application Number
- CN202411080308.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-08
AI Technical Summary
The existing nylon 12T preparation process has low mechanical properties and is difficult to meet the requirements of wind power blades.
High-pressure prepolymerization-low-pressure polymerization-atmospheric insulation-solid phase polycondensation process is adopted, and calcium carbonate of different particle sizes is added as a nucleating agent during the nylon 12T polymerization process to improve the crystallization structure and improve the strength and toughness of the material.
Through this process, the strength, toughness and thermal stability of nylon 12T are significantly improved, meeting the mechanical performance requirements of wind power blades, simplifying the process flow and reducing production costs.
Smart Images

Figure FSCQEVI2B6XJGHRWAHG3GFHSOCGGOWLH5UKOAXNU 
Figure GLWIKASLX8SPFYYZJOPISXS39G4QDJLDDZYDXTEQ
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polymer material preparation, and specifically relates to nylon 12T and a preparation method and application thereof. Background Art
[0002] The principle of wind power is that the wind rotor blades generate aerodynamic force under the action of wind to rotate the wind rotor, convert wind energy into mechanical energy, and finally generate electricity. The device for wind power generation is called a wind turbine, which is mainly composed of wind turbine blades, transmission system, generator, energy storage equipment, tower and electrical system. Among them, wind turbine blades are an important part of wind turbine generator sets and are the key to obtaining wind energy. Excellent quality and excellent performance are key factors to ensure the stable operation of the unit and capture wind energy. The changing application environment and 20-year service life put forward many requirements for the blades.
[0003] One of the keys to making blades larger is the design of the blade shape. Currently, blade materials use traditional thermosetting resins (epoxy, vinyl, etc.), which require that products be molded in one go as much as possible to reduce the number of parts. Adjacent parts are connected by adhesives. The complicated process increases production costs, so using thermosetting resins will lead to increased costs.
[0004] Nylon 12T resin is a thermoplastic engineering plastic with excellent performance, which has important applications in the fields of electrical appliances, automobiles, electronics, construction, wind power, etc. At present, in order to cope with the problems caused by the large-scale development of wind turbine blades, countries have focused on solving the problem of nylon 12T thermoplastic composite materials. However, the current preparation process of nylon 12T is not mature, and there are usually technical problems with low mechanical properties, which makes it difficult to meet the requirements of polyamide technology for wind turbine blades. Summary of the invention
[0005] The purpose of the present invention is to provide a nylon 12T and a preparation method and application thereof in view of the defects of the prior art. The preparation method has strong operability, and by adding calcium carbonate nucleating agents of different particle sizes, in addition to improving the performance of nylon 12T and shortening the reaction time, the strength and toughness of nylon 12T are fundamentally improved, meeting the use requirements of polyamide for wind turbine blades.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A method for preparing nylon 12T comprises the following steps:
[0008] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0009] (2) 100 parts by weight of nylon 12T salt, a catalyst, a molecular weight regulator and a nucleating agent are added to a reactor, the reactor is protected by inert gas, the temperature is raised to 200-230°C, and the reaction is carried out at a pressure of 2.0-2.4 MPa for 1-2 hours; the nucleating agent is composed of 0.2-0.5 parts by weight of small-particle calcium carbonate with an average particle size D50 of 100-200 nm and 0.8-1.3 parts by weight of large-particle calcium carbonate with an average particle size D50 of 700-1200 nm, and the average particle size D50 is the volume average particle size measured by laser scattering method;
[0010] (3) Release the pressure to 1.3-1.5 MPa and react at 170-190°C for 0.5-1h;
[0011] (4) Reduce to normal pressure and keep warm for 1-2 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0012] (5) The nylon 12T prepolymer powder is transferred to a solid phase polymerization reactor, vacuumed, and reacted at 160-200°C for 2-4 hours; then the temperature is raised to 220-250°C and the reaction is continued for 5-10 hours, cooled, and discharged to obtain nylon 12T with high mechanical properties.
[0013] As a commonly used engineering plastic, nylon 12T has both a crystal region with a tightly arranged molecular chain and an amorphous region with a disordered molecular chain arrangement in its microstructure. The crystal structure mainly provides high stiffness, high strength, creep resistance, and high temperature thermal stability for the material because of its dense structure and strong intermolecular interaction. The amorphous region gives the material certain impact resistance and elongation at break because of the mobility of its random chain structure. The crystallization behavior of nylon 12T will affect its comprehensive performance in all aspects. The prior art usually regulates the crystallization process of nylon 12T by adding a single nucleating agent such as silica and talcum powder to obtain a high-performance nylon 12T composite material. The inventor has also used silica of different particle sizes to prepare polymer microspheres in emulsion in previous work. However, nucleating agents such as silica and talcum powder have the technical problem of easy agglomeration in the nylon polymerization process, and the preparation process of nucleating agents such as nano-sized silica and talcum powder is complicated, which is not conducive to the industrial production of nylon.
[0014] The present invention improves the crystallization process of nylon 12T by adding small-particle calcium carbonate with an average particle size D50 of 100-200nm and large-particle calcium carbonate with an average particle size D50 of 700-1200nm as nucleating agents during the polymerization of nylon 12T. Generally speaking, small-particle nucleating agents are conducive to the formation of microcrystalline structures; however, if the particle size is too small, it is easy to cause inorganic fillers to agglomerate; and if the particle size is too large, it is not conducive to the formation of nylon microcrystalline structures. By adding two different sizes of calcium carbonate particles, not only the dispersion performance of calcium carbonate is promoted, but also the crystal structure of nylon 12T can be improved, the growth of microcrystals and the refinement of grains can be promoted, and then the hardness, strength, modulus, toughness, thermal stability and dimensional stability of the material are improved, which is also the root cause of the simultaneous improvement of strength and toughness in subsequent mechanical properties.
[0015] At the same time, the present invention improves the molecular weight of nylon 12T through high-pressure prepolymerization-low-pressure polymerization-normal pressure insulation-solid phase polycondensation process. Compared with the common high-pressure polymerization-solid phase polycondensation process in the prior art, the present invention reacts for 0.5-1h under the conditions of 1.3-1.5MPa and 170-190°C. This process can not only promote the growth of the molecular chain, but also facilitate the nucleating effect of calcium carbonate nucleating agents of different particle sizes. If the polymerization temperature is too low, it is difficult for the molecular chain to overcome the potential energy to undergo polymerization reaction; if the temperature is too high, it is easy to cause excessive growth of the molecular chain, and the nucleating agent has no time to play a role, and grows into large-sized grains, which is not conducive to the improvement of the mechanical properties of nylon 12T.
[0016] In one embodiment, the catalyst is one or more of hypophosphorous acid, sodium hypophosphite, potassium hypophosphite, lithium hypophosphite, magnesium hypophosphite, and calcium hypophosphite.
[0017] In one embodiment, the molecular weight regulator in step (2) is one or more of a monobasic acid or a dibasic acid.
[0018] In one embodiment, the molecular weight regulator in step (2) is one or more of benzoic acid, adipic acid, and acetic acid.
[0019] In one embodiment, in step (3), the pressure is released to 1.3-1.5 MPa within 10-30 min.
[0020] In one embodiment, the inert gas in step (2) is one or more of nitrogen and argon.
[0021] In one embodiment, the amounts of the catalyst and the molecular weight regulator used in step (2) are 0.1-1.2 parts by weight and 0.5-1 parts by weight, respectively.
[0022] In one embodiment, the large-particle calcium carbonate in step (2) is 0.9-1.2 parts by weight, and the average particle size D50 is 800-1000 nm.
[0023] Another aspect of the present invention provides nylon 12T and its application in the field of wind power.
[0024] Compared with the existing technology, the present invention has the following advantages: the present invention improves the molecular weight of nylon 12T through high-pressure prepolymerization-low-pressure polymerization-normal pressure insulation-solid phase polycondensation process, which not only promotes the growth of molecular chains, but also facilitates the nucleation of calcium carbonate nucleating agents of different particle sizes. The present invention improves the crystallization process of nylon 12T by adding small-particle calcium carbonate with an average particle size D50 of 100-200nm and large-particle calcium carbonate with an average particle size D50 of 700-1200nm as nucleating agents during the polymerization process of nylon 12T without coupling modification. By adding two calcium carbonate particles of different sizes, not only the dispersion performance of calcium carbonate is promoted, but also the crystal structure of nylon 12T can be improved, the growth of microcrystals and the refinement of grains can be promoted, and the strength and toughness of the material can be improved. DETAILED DESCRIPTION
[0025] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0026] Example 1
[0027] A method for preparing nylon 12T comprises the following steps:
[0028] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0029] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 200°C, and the reaction was carried out at a pressure of 2.0 MPa for 2 hours; the nucleating agent was composed of 0.2 parts by weight of small-particle calcium carbonate with an average particle size D50 of 100 nm and 0.9 parts by weight of large-particle calcium carbonate with an average particle size D50 of 800 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.3 parts by weight and 0.5 parts by weight respectively;
[0030] (3) Release the pressure to 1.5 MPa within 10 min and react at 170 °C for 1 h;
[0031] (4) Reduce to normal pressure, keep warm for 1 hour, discharge the material, and obtain nylon 12T prepolymer powder;
[0032] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 160°C for 4 h; then the temperature was raised to 220°C and the reaction was continued for 10 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0033] Example 2
[0034] A method for preparing nylon 12T comprises the following steps:
[0035] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0036] (2) 100 parts by weight of nylon 12T salt, catalyst potassium hypophosphite, molecular weight regulator acetic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 230°C, and the reaction was carried out at a pressure of 2.4 MPa for 1 hour; the nucleating agent was composed of 0.5 parts by weight of small-particle calcium carbonate with an average particle size D50 of 200 nm and 1.2 parts by weight of large-particle calcium carbonate with an average particle size D50 of 1000 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 1.2 parts by weight and 1 part by weight respectively;
[0037] (3) Release the pressure to 1.3 MPa within 30 min and react at 190 °C for 0.5 h;
[0038] (4) Reduce to normal pressure, keep warm for 2 hours, discharge the material, and obtain nylon 12T prepolymer powder;
[0039] (5) The nylon 12T prepolymer powder is transferred to a solid phase polymerization reactor, vacuumed, and reacted at 200°C for 2 hours; then the temperature is raised to 250°C and the reaction is continued for 5 hours, cooled, and discharged to obtain nylon 12T with high mechanical properties.
[0040] Example 3
[0041] A method for preparing nylon 12T comprises the following steps:
[0042] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0043] (2) 100 parts by weight of nylon 12T salt, catalyst calcium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 200°C, and the reaction was carried out at a pressure of 2.4 MPa for 2 hours; the nucleating agent was composed of 0.2 parts by weight of small-particle calcium carbonate with an average particle size D50 of 200 nm and 1.2 parts by weight of large-particle calcium carbonate with an average particle size D50 of 800 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.5 parts by weight and 0.5 parts by weight respectively;
[0044] (3) Release the pressure to 1.5 MPa within 30 min and react at 190 °C for 0.5 h;
[0045] (4) Reduce to normal pressure, keep warm for 2 hours, discharge the material, and obtain nylon 12T prepolymer powder;
[0046] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 160°C for 2 h; then the temperature was raised to 250°C and the reaction was continued for 10 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0047] Example 4
[0048] A method for preparing nylon 12T comprises the following steps:
[0049] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0050] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 230°C, and the reaction was carried out at a pressure of 2.0 MPa for 1 hour; the nucleating agent was composed of 0.5 parts by weight of small-particle calcium carbonate with an average particle size D50 of 100 nm and 0.9 parts by weight of large-particle calcium carbonate with an average particle size D50 of 1000 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 1.2 parts by weight and 0.5 parts by weight respectively;
[0051] (3) Release the pressure to 1.3 MPa within 10 min and react at 170 °C for 0.5 h;
[0052] (4) Reduce to normal pressure, keep warm for 1 hour, discharge the material, and obtain nylon 12T prepolymer powder;
[0053] (5) The nylon 12T prepolymer powder is transferred to a solid phase polymerization reactor, vacuumed, and reacted at 200°C for 2 hours; then the temperature is raised to 220°C and the reaction is continued for 5 hours, cooled, and discharged to obtain nylon 12T with high mechanical properties.
[0054] Example 5
[0055] A method for preparing nylon 12T comprises the following steps:
[0056] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0057] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 210°C, and the reaction was carried out at a pressure of 2.1 MPa for 1.2 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 130 nm and 1 part by weight of large-particle calcium carbonate with an average particle size D50 of 850 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.6 parts by weight and 0.7 parts by weight respectively;
[0058] (3) Release the pressure to 1.4 MPa within 20 min and react at 176 °C for 0.6 h;
[0059] (4) Reduce to normal pressure and keep warm for 1.1 hours, then discharge to obtain nylon 12T prepolymer powder;
[0060] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 170°C for 3.4 hours; then the temperature was raised to 230°C and the reaction was continued for 8 hours. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0061] Example 6
[0062] A method for preparing nylon 12T comprises the following steps:
[0063] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0064] (2) 100 parts by weight of nylon 12T salt, catalyst calcium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 220°C, and the reaction was carried out at a pressure of 2.3 MPa for 1.7 hours; the nucleating agent was composed of 0.4 parts by weight of small-particle calcium carbonate with an average particle size D50 of 190 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 950 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 1.1 parts by weight and 0.9 parts by weight respectively;
[0065] (3) Depressurize to 1.3 MPa after 22 min and react at 188 °C for 0.6 h;
[0066] (4) Reduce to normal pressure and keep warm for 1.7 hours, then discharge to obtain nylon 12T prepolymer powder;
[0067] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 190°C for 2.6 hours; then the temperature was raised to 240°C and the reaction was continued for 7 hours. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0068] Example 7
[0069] A method for preparing nylon 12T comprises the following steps:
[0070] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0071] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.1 MPa for 1.3 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 160 nm and 0.9 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.7 parts by weight and 0.8 parts by weight respectively;
[0072] (3) Release the pressure to 1.4 MPa after 30 min and react at 184 °C for 0.7 h;
[0073] (4) Reduce to normal pressure and keep warm for 1.8 hours, then discharge to obtain nylon 12T prepolymer powder;
[0074] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 170°C for 2.4 hours; then the temperature was raised to 235°C and the reaction was continued for 6 hours. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0075] Example 8
[0076] A method for preparing nylon 12T comprises the following steps:
[0077] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0078] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0079] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0080] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0081] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0082] Example 9
[0083] A method for preparing nylon 12T comprises the following steps:
[0084] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0085] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm and 0.8 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0086] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0087] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0088] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0089] Example 10
[0090] A method for preparing nylon 12T comprises the following steps:
[0091] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0092] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm and 1.3 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0093] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0094] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0095] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0096] Embodiment 11
[0097] A method for preparing nylon 12T comprises the following steps:
[0098] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0099] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 700 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0100] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0101] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0102] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0103] Example 12
[0104] A method for preparing nylon 12T comprises the following steps:
[0105] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0106] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 1200 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0107] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0108] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0109] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0110] Comparative Example 1
[0111] A method for preparing nylon 12T comprises the following steps:
[0112] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0113] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 1.4 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm, and the average particle size D50 was the volume average particle size determined by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0114] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0115] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0116] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0117] Comparative Example 2
[0118] A method for preparing nylon 12T comprises the following steps:
[0119] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0120] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 1.4 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0121] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0122] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge to obtain nylon 12T prepolymer powder;
[0123] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0124] Comparative Example 3
[0125] A method for preparing nylon 12T comprises the following steps:
[0126] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0127] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.08 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0128] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0129] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0130] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0131] Comparative Example 4
[0132] A method for preparing nylon 12T comprises the following steps:
[0133] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0134] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.8 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0135] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0136] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0137] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0138] Comparative Example 5
[0139] A method for preparing nylon 12T comprises the following steps:
[0140] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0141] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 60 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0142] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0143] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0144] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0145] Comparative Example 6
[0146] A method for preparing nylon 12T comprises the following steps:
[0147] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0148] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 300 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0149] (3) Release the pressure to 1.4 MPa after 20 min and react at 180 °C for 0.7 h;
[0150] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0151] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0152] Comparative Example 7
[0153] A method for preparing nylon 12T comprises the following steps:
[0154] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0155] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0156] (3) Release the pressure to 1.4 MPa after 20 min and react at 160 °C for 0.7 h;
[0157] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0158] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 h; then the temperature was raised to 235°C and the reaction was continued for 7 h. The mixture was cooled and discharged to obtain nylon 12T with high mechanical properties.
[0159] Comparative Example 8
[0160] A method for preparing nylon 12T comprises the following steps:
[0161] (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials;
[0162] (2) 100 parts by weight of nylon 12T salt, catalyst sodium hypophosphite, molecular weight regulator benzoic acid and nucleating agent were added to a reactor, nitrogen was filled for protection, the temperature was raised to 215°C, and the reaction was carried out at a pressure of 2.2 MPa for 1.5 hours; the nucleating agent was composed of 0.3 parts by weight of small-particle calcium carbonate with an average particle size D50 of 150 nm and 1.1 parts by weight of large-particle calcium carbonate with an average particle size D50 of 900 nm, and the average particle size D50 was the volume average particle size measured by laser scattering method; the amounts of catalyst and molecular weight regulator were 0.8 parts by weight and 0.7 parts by weight respectively;
[0163] (3) Release the pressure to 1.4 MPa after 20 min and react at 205 °C for 0.7 h;
[0164] (4) Reduce to normal pressure and keep warm for 1.5 hours, then discharge the material to obtain nylon 12T prepolymer powder;
[0165] (5) The nylon 12T prepolymer powder was transferred to a solid phase polymerization reactor, vacuumed, and reacted at 180°C for 3 hours; then the temperature was raised to 235°C and the reaction was continued for 7 hours, cooled, and discharged to obtain high mechanical property nylon 12T. The high mechanical property nylon 12T prepared according to the above method was injection molded into a standard specimen on an injection molding machine, and its mechanical properties were tested. The tensile strength (MPa) and elongation at break (%) were tested according to ISO527-2 standard; the flexural strength (MPa) was tested according to ISO178 standard; the notched impact strength (kJ / m2) was tested according to ISO179-1 standard; the test results are shown in Tables 1 to 3.
[0166]
[0167]
[0168] As can be seen from Examples 1-12, the present invention improves the molecular weight of nylon 12T through high-pressure prepolymerization-low-pressure polymerization-normal pressure insulation-solid phase polycondensation process, and improves the crystallization process of nylon 12T by adding small-particle calcium carbonate with an average particle size D50 of 100-200nm and large-particle calcium carbonate with an average particle size D50 of 700-1200nm as nucleating agents during the polymerization of nylon 12T, and the strength and toughness of the mechanical properties are simultaneously improved. Specifically, as can be seen from Examples 8-12, the present invention adds a small amount of small-particle nucleating agent to a large-particle nucleating agent in a large amount, improves the dispersion of the nucleating agent, and is conducive to the uniform nucleation process during the polymerization of nylon monomers, wherein the large particle size is relatively large and dispersed more evenly, and the impact on the performance is relatively small relative to the small particle nucleating agent. Among them, when the large particle size calcium carbonate is 0.9-1.2 parts by weight and the average particle size D50 is 800-1000nm, the mechanical properties of the prepared nylon 12T are the best.
[0169] It can be seen from Example 8 and Comparative Examples 1-8 that the size and dosage of the small particle size nucleating agent and the prepolymerization temperature have a great influence on the performance. When the particle size of small particle size calcium carbonate is too small or the dosage is too much, the dispersion is uneven, which easily leads to agglomeration of inorganic filler; while the particle size is too large or the dosage is too small, it is not conducive to the formation of nylon microcrystalline structure, and when the dosage of small particle size calcium carbonate is small, it is not conducive to the dispersion of large particle size calcium carbonate. At the same time, the prepolymerization temperature of 170-190°C can promote the growth of molecular chains, which is conducive to the nucleation effect of calcium carbonate nucleating agents of different particle sizes. If the polymerization temperature is too low, it is difficult for the molecular chain to overcome the potential energy to undergo polymerization reaction; if the temperature is too high, it is easy to cause excessive growth of molecular weight, and the nucleating agent has no time to play a role, and it grows into large-sized grains, which is not conducive to the improvement of the mechanical properties of nylon 12T.
[0170] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing nylon 12T, It is characterized in that The following steps are involved: (1) Preparation of nylon 12T salt using dodecyl diamine and terephthalic acid as raw materials; (2) 100 parts by weight of nylon 12T salt, a catalyst, a molecular weight regulator and a nucleating agent are added to a reactor, the reactor is protected by inert gas, the temperature is raised to 200-230°C, and the reaction is carried out at a pressure of 2.0-2.4 MPa for 1-2 hours; the nucleating agent is composed of 0.2-0.5 parts by weight of small-particle calcium carbonate with an average particle size D50 of 100-200 nm and 0.8-1.3 parts by weight of large-particle calcium carbonate with an average particle size D50 of 700-1200 nm, and the average particle size D50 is the volume average particle size measured by laser scattering method; (3) Release the pressure to 1.3-1.5 MPa and react at 170-190°C for 0.5-1h; (4) Reduce to normal pressure and keep warm for 1-2 hours, then discharge the material to obtain nylon 12T prepolymer powder; (5) The nylon 12T prepolymer powder is transferred to a solid phase polymerization reactor, vacuumed, and reacted at 160-200°C for 2-4 hours; then the temperature is raised to 220-250°C and the reaction is continued for 5-10 hours, cooled, and discharged to obtain nylon 12T.
2. A method for preparing nylon 12T as claimed in claim 1, It is characterized in that The catalyst in step (2) is one or more of hypophosphorous acid, sodium hypophosphite, potassium hypophosphite, lithium hypophosphite, magnesium hypophosphite and calcium hypophosphite.
3. A method for preparing nylon 12T as claimed in claim 1, It is characterized in that In step (2), the molecular weight regulator is one or more of a monobasic acid or a dibasic acid.
4. A method for preparing nylon 12T as claimed in claim 3, It is characterized in that In step (2), the molecular weight regulator is one or more of benzoic acid, adipic acid and acetic acid.
5. A method for preparing nylon 12T as claimed in claim 1, It is characterized in that In step (3), the pressure is released to 1.3-1.5 MPa within 10-30 minutes.
6. A method for preparing nylon 12T as claimed in claim 1, It is characterized in that In step (2), the inert gas is one or more of nitrogen and argon.
7. A method for preparing nylon 12T as claimed in claim 1, It is characterized in that In step (2), the amounts of catalyst and molecular weight regulator are 0.1-1.2 parts by weight and 0.5-1 parts by weight respectively.
8. A method for preparing nylon 12T as claimed in claim 1, It is characterized in that In step (2), the large-particle calcium carbonate is 0.9-1.2 parts by weight, and the average particle size D50 is 800-1000 nm.
9. A nylon 12T, It is characterized in that The nylon 12T is prepared by the preparation method of any one of claims 1 to 8.
10. Application of nylon 12T as claimed in claim 9 in the field of wind power.
Citation Information
Cited By
High-strength flame-retardant high-temperature PA12T composite material and preparation method thereof