A high-strength anti-corrosion coating for oil casing and preparation method thereof
By using hollow structural coatings of modified graphene and nickel-based alloys on the oil casing, the serious corrosion problem of oil casing under corrosive media is solved, the corrosion resistance and mechanical properties are improved, the service life is extended and the wear is reduced. .
Patent Information
- Application Number
- CN202410819012.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-06-24
AI Technical Summary
Oil casing is prone to severe corrosion when it comes into contact with corrosive media for a long time, resulting in hysteresis of production operations or scrapping of wells. The existing anti-corrosion measures are not effective.
Using an oil casing high-strength anticorrosion coating, including modified graphene, nickel-based alloy and surfactant, the nickel-based alloy and oleophobic modified graphene is formed to form covalent connections and fill it with modified graphite. Ethylene into nickel-based alloys to enhance corrosion resistance and mechanical properties.
It significantly improves the corrosion resistance, mechanical properties and wear resistance of nickel-based alloys, extends the service life of the coating, reduces wear and corrosion damage, and enhances the overall strength and toughness of the material.
Smart Images

Figure BDA0004908589030000071 
Figure BDA0004908589030000081 
Figure BDA0004908589030000111
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of anti-corrosion coatings, and in particular to a high-strength anti-corrosion coating for oil casing and a preparation method thereof. Background Art
[0002] Oil casing is a kind of pipeline used in oil and gas wells such as petroleum and natural gas, mainly used for transporting oil and gas or injecting water and gas. Its characteristics include high pressure resistance, corrosion resistance, wear resistance, etc., and it can operate stably for a long time in harsh working environments. Oil casing is usually made of carbon steel, alloy steel and other materials, with high strength and durability. In addition, oil casing also has good sealing performance, which can effectively prevent oil and gas leakage and ensure the safety and stability of underground operations.
[0003] The corrosion of products such as oil casing and tubing mainly occurs in two links: the first is atmospheric corrosion during transportation and storage, especially in high temperature, high humidity and high salt environment; the second is corrosion by corrosive media (such as H2S, CO2 and SRB, etc.) in the application environment. The corrosion damage of oil casing and tubing will cause delays and suspension of production operations at the least, and will lead to major economic losses and serious environmental damage accidents such as the scrapping of oil and gas wells at the worst. Since the inner wall of oil casing and tubing often needs to be in contact with various corrosive media for a long time, the corrosion of the inner wall is particularly common and serious, and internal corrosion protection is more urgent and important. For this reason, we provide a high-strength anti-corrosion coating for oil casing and tubing and a preparation method to solve the above problems. Summary of the invention
[0004] The purpose of the present invention is to make up for the deficiencies of the prior art and to provide a high-strength anti-corrosion coating for oil casing and a preparation method thereof, which solves the problem of serious corrosion of oil casing due to long-term contact with corrosive media.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a high-strength anti-corrosion coating for oil casing, comprising modified graphene, a nickel-based alloy, a solvent and a surfactant.
[0006] The modified graphene, the nickel-based alloy, the solvent and the surfactant are composed of the following weight percentages: 5%-10% of modified graphene, 70%-90% of nickel-based alloy, 10%-20% of solvent and 1%-2% of surfactant.
[0007] The nickel-based alloy is nanoparticles with a hollow structure, the modified graphene is oleophobic modified graphene, and the solvent is either ethanol or acetone.
[0008] The modified graphene can be prepared by a covalent bonding method, and the particle size of the modified graphene is 50nm to 300nm.
[0009] The mass fractions of the elements in the nickel-based alloy are as follows: C: 0.7%-1.1%, B: 3.0%-4.0%, Si: 3.5%-5.0%, Cr: 17.0%-20.0%, Cu: 0-0.5%, Fe: 0-5%, Mo: 2.0%-3.0%, rare earth: 2.0%-3.0%, and the balance is Ni and unavoidable impurities.
[0010] The preparation steps of the above-mentioned high-strength anti-corrosion coating for oil casing are as follows:
[0011] Step A, preparing the nickel-based alloy into nanoparticles: crushing and grinding the nickel-based alloy, placing the alloy powder in a high-temperature furnace, and forming nano-scale nickel-based alloy particles at 800° C.-1000° C. by chemical vapor deposition or physical vapor deposition.
[0012] Step B, forming a hollow structure of the nickel-based alloy: placing the nano-scale nickel-based alloy prepared in step A in a specific template, immersing the template and the nickel-based alloy in an acidic or alkaline solution, the ions in the solution react with the surface of the template to form holes on the surface of the template, and sintering the nickel-based alloy with holes at a high temperature to solidify the nickel-based alloy and form a hollow structure.
[0013] Step C, filling modified graphene: modifying the graphene, and filling the modified graphene into the hollow structure of the nickel-based alloy through surface modification treatment to obtain an anti-corrosion coating.
[0014] Step D, coating: coating the prepared anti-corrosion coating on the surface of the oil casing, drying the coated coating, and then curing the coating to firmly bond the coating to the metal substrate.
[0015] In step B, the specific template is polystyrene microspheres, the reaction time between the template and the nickel-based alloy nanoparticles is 6-10 hours, the sintering temperature of the high-temperature sintering is 800° C.-1200° C., and the sintering time is 9-16 hours.
[0016] In step C, the modification and filling method of graphene is as follows:
[0017] Step C-1, functionalizing the graphene to introduce functional groups suitable for covalent bonding, and the preferred functionalization method is either reduction of graphene oxide or conversion of functional groups on graphene oxide.
[0018] Step C-2, introducing an activation group on the functionalized graphene surface, reacting the molecule containing the oleophobic group with the activated graphene surface to form a covalent connection.
[0019] Step C-3, purifying and characterizing the covalently linked graphene to ensure that the oleophobic groups are successfully linked to the graphene surface.
[0020] Step C-4, adding the modified graphene powder into a solvent, and adding an appropriate amount of a surfactant, dispersing the graphene in the solution by ultrasonic treatment or stirring to prepare a uniform graphene dispersion.
[0021] Step C-5, pouring the prepared graphene dispersion into the nickel-based alloy with a hollow structure, ensuring that the material is completely covered and impregnated, and performing an impregnation treatment so that the graphene fully penetrates into the nickel-based alloy with a hollow structure.
[0022] In step C-5, the sample after immersion is dried, and the residual solvent can be removed by natural air drying or heating drying.
[0023] Compared with the prior art, the high-strength anti-corrosion coating for oil casing and the preparation method thereof have the following beneficial effects:
[0024] 1. The present invention can improve the corrosion resistance of the nickel-based alloy by adding modified graphene to the nickel-based alloy with a hollow structure. At the same time, the nickel-based alloy with a hollow structure has a larger specific surface area, which can increase the contact area between the material and the environment, which is beneficial to enhancing the reaction activity and catalytic performance of the material. Filling the modified graphene in the nickel-based alloy with a hollow structure can enhance the mechanical properties of the material, improve the strength and toughness of the material, and further improve the overall strength of the anti-corrosion coating.
[0025] 2. The present invention prepares a nickel-based alloy with a hollow structure, which has a lighter weight than a solid structure, is beneficial to reducing the density of the material and improving the specific strength and specific stiffness of the material. At the same time, the hollow structure has a shorter mass transfer path, which is beneficial to the mass transfer process and improves the mass transfer performance and response speed of the material. In addition, the surface area of the nickel-based alloy with a hollow structure is increased, and the oxidation reaction proceeds more evenly on the entire surface, so that the thickness and uniformity of the oxide film are better, thereby improving the corrosion resistance of the nickel-based alloy.
[0026] 3. The present invention performs oleophobic modification on graphene to make it oleophobic, which can effectively prevent the penetration of water and corrosive media, thereby enhancing the anti-corrosion performance of the coating, helping to extend the service life of the coating and improve the anti-corrosion effect. At the same time, the addition of oleophobic modified graphene can increase the hardness and wear resistance of the coating, reduce the degree of wear of the coating, and graphene also has excellent chemical stability, which can further enhance the corrosion resistance of the coating and resist the erosion of corrosive media.
[0027] 4. Compared with physical mixing, chemical reduction and chemical vapor deposition, the present invention fills graphene in a hollow structured nickel-based alloy. The hollow structured nanoparticles provide a more stable structural support, which, combined with the filling structure of graphene, can improve the performance stability and cycle stability of the material. At the same time, filling graphene in a hollow structured nickel-based alloy can achieve more uniform distribution and filling, ensure good bonding between graphene and the matrix, and improve the performance stability of the material.
[0028] 5. The present invention connects molecules containing oleophobic groups to the graphene surface by covalent bonding. The molecules of the oleophobic groups can be firmly connected to the graphene surface to form stable chemical bonds, which can prevent the oleophobic groups from falling off the graphene surface during use, thereby improving its stability and durability. At the same time, by covalently bonding molecules containing oleophobic groups to the graphene surface, the anti-pollution performance of graphene can be improved, the possibility of dirt adhesion can be reduced, and the service life of graphene can be extended.
[0029] Other advantages, objectives and features of the present invention will be set forth in part in the following description and, in part, will be apparent to those skilled in the art based on an examination of the following or may be taught from the practice of the present invention. DETAILED DESCRIPTION
[0030] The following will be combined with the table of the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Embodiment 1: A high-strength anti-corrosion coating for oil casing, comprising modified graphene, a nickel-based alloy, a solvent and a surfactant.
[0032] Among them, the modified graphene, nickel-based alloy, solvent and surfactant are composed of the following weight percentages: 5%-10% of modified graphene, 70%-90% of nickel-based alloy, 10%-20% of solvent, and 1%-2% of surfactant; the nickel-based alloy is nanoparticles with a hollow structure, the modified graphene is oleophobic modified graphene, and the solvent is either ethanol or acetone; the present invention can improve the corrosion resistance of the nickel-based alloy by adding the modified graphene to the nickel-based alloy with a hollow structure, and at the same time, the nickel-based alloy with a hollow structure has a larger specific surface area, which can increase the contact area between the material and the environment, which is beneficial to enhancing the reaction activity and catalytic performance of the material, and filling the modified graphene in the nickel-based alloy with a hollow structure can enhance the mechanical properties of the material, improve the strength and toughness of the material, and can further improve the overall strength of the anti-corrosion coating.
[0033] The above-mentioned modified graphene can be prepared by a covalent bonding method, and the modified graphene particle size is 150nm; the present invention performs oleophobic modification on graphene to make the graphene oleophobic, which can effectively prevent the penetration of water and corrosive media, thereby enhancing the anti-corrosion performance of the coating, helping to extend the service life of the coating and improve the anti-corrosion effect. At the same time, the addition of oleophobic modified graphene can increase the hardness and wear resistance of the coating, reduce the degree of wear of the coating, and the graphene also has excellent chemical stability, which can further enhance the corrosion resistance of the coating and resist the erosion of corrosive media.
[0034] The mass fraction of each element in the above-mentioned nickel-based alloy is: C: 0.7% ~ 1.1%, B: 3.0% ~ 4.0%, Si: 3.5% ~ 5.0%, Cr: 17.0% ~ 20.0%, Cu: 0 ~ 0.5%, Fe: 0 ~ 5%, Mo: 2.0% ~ 3.0%, rare earth: 2.0% ~ 3.0%, and the balance is Ni and unavoidable impurities.
[0035] The preparation method of the high-strength anti-corrosion coating for oil casing comprises the following steps:
[0036] Step A, preparing the nickel-based alloy into nanoparticles: crushing and grinding the nickel-based alloy, placing the alloy powder in a high-temperature furnace, and forming nano-scale nickel-based alloy particles at 800° C.-1000° C. by chemical vapor deposition or physical vapor deposition.
[0037] Step B, forming a hollow structure of the nickel-based alloy: placing the nano-scale nickel-based alloy prepared in step A in a specific template, immersing the template and the nickel-based alloy in an acidic or alkaline solution, the ions in the solution react with the surface of the template to form holes on the surface of the template, sintering the nickel-based alloy treated with holes at a high temperature to solidify the nickel-based alloy and form a hollow structure; the specific template is a polystyrene microsphere, the reaction time between the template and the nickel-based alloy nanoparticles is 7 hours, the sintering temperature of the high-temperature sintering is 950° C., and the sintering time is 10 hours; the nickel-based alloy with a hollow structure prepared by the present invention has a lighter weight than a solid structure, is conducive to reducing the density of the material, and improves the specific strength and specific stiffness of the material. At the same time, the hollow structure has a shorter mass transfer path, which is conducive to the mass transfer process, improves the mass transfer performance and response speed of the material, and the surface area of the nickel-based alloy with a hollow structure is increased, and the oxidation reaction is carried out more uniformly on the entire surface, so that the thickness and uniformity of the oxide film are better, thereby improving the corrosion resistance of the nickel-based alloy.
[0038] Step C, filling modified graphene: modifying graphene, and filling the modified graphene into the hollow structure of the nickel-based alloy through surface modification to obtain an anti-corrosion coating; wherein the surface modification is a method of electrochemical deposition or solution impregnation; the present invention fills graphene into the nickel-based alloy with a hollow structure, and compared with physical mixing, chemical reduction and chemical vapor deposition, the nanoparticles of the hollow structure provide a more stable structural support, which, combined with the filling structure of the graphene, can improve the performance stability and cycle stability of the material. At the same time, filling the nickel-based alloy with a hollow structure with graphene can achieve more uniform distribution and filling, ensure good combination of graphene and the matrix, and improve the performance stability of the material.
[0039] Step D, coating: coating the prepared nickel-based alloy-modified graphene anti-corrosion coating on the surface of the oil casing, drying the coated coating, and then curing it to firmly bond the coating to the metal substrate.
[0040] In step C, the modification and filling method of graphene is as follows:
[0041] Step C-1, functionalizing the graphene to introduce functional groups suitable for covalent bonding, wherein the preferred functionalization method is either reduction of graphene oxide or conversion of functional groups on graphene oxide;
[0042] Step C-2, introducing an activation group on the functionalized graphene surface, reacting the molecule containing the oleophobic group with the activated graphene surface to form a covalent connection;
[0043] Step C-3, purifying and characterizing the covalently linked graphene to ensure that the oleophobic group is successfully linked to the graphene surface; the addition of oleophobic modified graphene can reduce the friction coefficient of the coating after it is prepared into a coating, reduce the friction loss on the coating surface, and improve the wear resistance and lubricity of the coating; the present invention connects the molecules containing the oleophobic group to the graphene surface by covalent linking, and the molecules of the oleophobic group can be firmly connected to the graphene surface to form a stable chemical bond, which can prevent the oleophobic group from falling off the graphene surface during use, thereby improving its stability and durability. At the same time, by covalently linking the molecules containing the oleophobic group to the graphene surface, the anti-pollution performance of the graphene can be improved, and the possibility of dirt adhesion can be reduced, thereby extending the service life of the graphene;
[0044] Step C-4, adding the modified graphene powder into a solvent, and adding an appropriate amount of a surfactant, dispersing the graphene in the solution by ultrasonic treatment or stirring to prepare a uniform graphene dispersion;
[0045] Step C-5, pouring the prepared graphene dispersion into the nickel-based alloy with a hollow structure to ensure that the material is completely covered and impregnated, and performing an impregnation treatment to allow the graphene to fully penetrate into the nickel-based alloy with a hollow structure; drying the impregnated sample, and the residual solvent can be removed by natural air drying or heat drying, and the dried sample is sintered to fix the graphene filling in the hollow structure of the nickel-based alloy, while improving the bonding strength and performance of the material.
[0046] Performance Test:
[0047] Table 1: Preparation materials and dosage table of test groups 1-4 and comparison group 1 in Example 1.
[0048]
[0049] The following performance tests were performed on the anti-corrosion coatings provided by test groups 1-4 and comparison group 1 of this application:
[0050] Detection method:
[0051] 1. Wear resistance The abrasion weight loss of the oil casing after the anti-corrosion coating prepared in this application is tested by using the standard of ASTM G65 "Standard test method for measuring wear using a dry sand / banana wheel apparatus".
[0052] 2. Corrosion resistance The corrosion rate of the oil casing after the anti-corrosion coating prepared in this application was measured using the standard of GB / T19746-2005 "Corrosion of metals and alloys in salt solution immersion test".
[0053] 3. The strength test adopts the standard of GB / T228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method" to detect the tensile strength and yield strength of the oil casing after the anti-corrosion coating prepared in this application is applied.
[0054] Performance test results:
[0055] Please refer to Table 2 for relevant data of performance test results.
[0056] Table 2: Performance test result data table of test groups 1-4 and comparison group 1 in Example 1.
[0057]
[0058] It can be seen from the test results that this embodiment increases the content of modified graphene in the coating and reduces the content of nickel-based alloy. Increasing the content of modified graphene helps to improve the mechanical properties of the coating and enhance the wear resistance of the coating. The surface of the nickel-based alloy in the coating will undergo an oxidation reaction with oxygen to form an oxide film. This oxide film is a dense, impermeable oxide layer that can effectively prevent oxygen and water molecules from further corroding the alloy matrix; at the same time, a small amount of modified graphene is doped, which can not only further improve the corrosion resistance of the nickel-based alloy, but also improve the wear resistance of the alloy, reduce the loss of the alloy under friction and wear conditions, and improve the strength and hardness of the alloy, and increase the tensile and compressive properties of the alloy.
[0059] In the coating, modified graphene and nickel-based alloy each have an addition threshold. It can be seen from the test results of test group 1 and test group 2 that when the content of modified graphene is 5%, the content of nickel-based alloy is reduced, and the relative content of modified graphene in test group 1 is reduced relative to the relative content of modified graphene in test group 2. Therefore, the wear resistance and corrosion resistance of the coating are improved, and the tensile strength and yield strength performance are reduced; it can be seen from the test results of test group 2 and test group 3 that when the content of nickel-based alloy is 80%, the content of modified graphene is increased to improve the performance of the coating; it can be seen from the test results of test group 3 and test group 4 that when the addition amount of modified graphene and nickel-based alloy is further adjusted, the performance of the coating will be greatly reduced.
[0060] Therefore, when the addition amount of modified graphene and the addition amount of nickel-based alloy are close to the addition threshold, the coating performance will change. From the proportion of preparation raw materials used in test group 3 and test group 4, it can be seen that the addition threshold of modified graphene is 8%-10%, and the addition threshold of nickel-based alloy is 70%-80%.
[0061] Example 2: Based on Example 1, a high-strength anti-corrosion coating for oil casing includes modified graphene, a nickel-based alloy, a solvent and a surfactant, wherein the modified graphene, the nickel-based alloy, the solvent and the surfactant are composed in the following weight percentages: 10% modified graphene, 75% nickel-based alloy, 14% solvent and 1% surfactant; the nickel-based alloy is a nanoparticle with a hollow structure, the modified graphene is an oleophobic modified graphene, and the solvent is either ethanol or acetone.
[0062] The modified graphene can be prepared by a covalent bonding method, and the particle size of the modified graphene is 270 nm.
[0063] The mass fraction of each element in the above-mentioned nickel-based alloy is: C: 1.1%, B: 4.0%, Si: 5.0%, Cr: 20.0%, Cu: 0.5%, Fe: 5%, Mo: 3.0%, rare earth: 3.0%, and the balance is Ni and inevitable impurities. By reducing the nickel content, the processing properties of the alloy can be improved, making the alloy easier to process and form. At the same time, reducing the nickel content can reduce the cost of the alloy and make the alloy more competitive.
[0064] The method for preparing the above-mentioned high-strength anti-corrosion coating for oil casing comprises the following steps:
[0065] Step A, preparing the nickel-based alloy into nanoparticles: crushing and grinding the nickel-based alloy, placing the alloy powder in a high-temperature furnace, and forming nano-scale nickel-based alloy particles at 800° C.-1000° C. by chemical vapor deposition or physical vapor deposition.
[0066] Step B, forming a hollow structure of the nickel-based alloy: placing the nano-scale nickel-based alloy prepared in step A in a specific template, immersing the template and the nickel-based alloy in an acidic or alkaline solution, the ions in the solution react with the surface of the template to form holes on the surface of the template, sintering the nickel-based alloy with holes at a high temperature to solidify the nickel-based alloy and form a hollow structure; the specific template is polystyrene microspheres, the reaction time of the template and the nickel-based alloy nanoparticles is 9 hours, the sintering temperature of the high-temperature sintering is 1150° C., and the sintering time is 15 hours.
[0067] Step C, filling modified graphene: modifying the graphene and filling the modified graphene into the hollow structure of the nickel-based alloy through surface modification to obtain an anti-corrosion coating; wherein the surface modification is a method of electrochemical deposition or solution impregnation.
[0068] Step D, coating: coating the prepared nickel-based alloy-modified graphene anti-corrosion coating on the surface of the oil casing, drying the coated coating, and then curing it to firmly bond the coating to the metal substrate.
[0069] In step C, the modification and filling method of graphene is as follows:
[0070] Step C-1, functionalizing the graphene to introduce functional groups suitable for covalent bonding, wherein the preferred functionalization method is either reduction of graphene oxide or conversion of functional groups on graphene oxide;
[0071] Step C-2, introducing an activation group on the functionalized graphene surface, reacting the molecule containing the oleophobic group with the activated graphene surface to form a covalent connection;
[0072] Step C-3, purifying and characterizing the covalently linked graphene to ensure that the oleophobic group is successfully linked to the graphene surface; the addition of oleophobic modified graphene can reduce the friction coefficient of the coating after it is prepared into a coating, reduce the friction loss on the coating surface, and improve the wear resistance and lubricity of the coating;
[0073] Step C-4, adding the modified graphene powder into a solvent, and adding an appropriate amount of a surfactant, dispersing the graphene in the solution by ultrasonic treatment or stirring to prepare a uniform graphene dispersion;
[0074] Step C-5, pouring the prepared graphene dispersion into the nickel-based alloy with a hollow structure to ensure that the material is completely covered and impregnated, and performing an impregnation treatment to allow the graphene to fully penetrate into the nickel-based alloy with a hollow structure; drying the impregnated sample, and the residual solvent can be removed by natural air drying or heat drying, and the dried sample is sintered to fix the graphene filling in the hollow structure of the nickel-based alloy, while improving the bonding strength and performance of the material.
[0075] Relevant performance tests of Example 2:
[0076] In Example 2, the raw materials and dosages used in the preparation of the anti-corrosion coating in each test group are shown in Table 3.
[0077] Table 3: Preparation materials and dosage table of test groups 5-8 and comparison group 2 in Example 2.
[0078]
[0079] The following performance tests were performed on the anti-corrosion coatings provided by test groups 5-8 and comparison group 2 of this application. For specific test data, see Table 4.
[0080] Detection method:
[0081] 1. Wear resistance The abrasion weight loss of the oil casing after the anti-corrosion coating prepared in this application is tested by using the standard of ASTM G65 "Standard test method for measuring wear using a dry sand / banana wheel apparatus".
[0082] 2. Corrosion resistance The corrosion rate of the oil casing after the anti-corrosion coating prepared in this application was measured using the standard of GB / T19746-2005 "Corrosion of metals and alloys in salt solution immersion test".
[0083] 3. The strength test adopts the standard of GB / T228.1-2010 "Tensile test of metallic materials Part 1: Room temperature test method" to detect the tensile strength and yield strength of the oil casing after the anti-corrosion coating prepared in this application is applied.
[0084] Table 4: Performance test result data table of test groups 5-8 and comparison group 2 in Example 2.
[0085]
[0086] According to the performance test data table in Table 4, it can be seen that: this embodiment further tests the addition threshold value of modified graphene and nickel-based alloy. In the test results, it can be seen from test groups 5, 6 and 7 that when the addition amount of modified graphene gradually increases and the addition amount of nickel-based alloy gradually decreases, the performance of the coating gradually increases. It can be seen from test groups 7 and 8 that when the content of modified graphene is 10%, further reducing the content of nickel-based alloy will reduce the performance of the coating. Therefore, when the content of modified graphene is 10% and the content of nickel-based alloy is 75%, the performance of the coating reaches the best.
[0087] It can be seen from test group 8 and comparison group 2 that when the amount of modified graphene added exceeds the addition threshold or the amount of nickel-based alloy added is lower than the addition threshold, the performance of the coating will be reduced; by further increasing the content of modified graphene in the coating and reducing the content of nickel-based alloy, graphene has excellent strength and stiffness. Filling it into nickel-based alloy can improve the strength, hardness and tensile resistance of the alloy, so that the nickel-based alloy has better wear resistance and tensile resistance. Graphene has excellent thermal conductivity. Filling it into nickel-based alloy can improve the overall thermal conductivity of the alloy, which helps to improve the heat dissipation effect and heat transfer speed of nickel-based alloy. Nickel-based alloy can further improve the oxidation reaction in high temperature environment, so that the oxide film is generated more quickly, further improving the corrosion resistance of the coating.
[0088] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. A high-strength anti-corrosion coating for oil casing, comprising modified graphene, nickel-based alloy, solvent and surfactant, Features: The modified graphene, the nickel-based alloy, the solvent and the surfactant are composed of the following weight percentages: 5%-10% of modified graphene, 70%-90% of nickel-based alloy, 10%-20% of solvent, and 1%-2% of surfactant, and the sum of the contents of the above components is 100%; The nickel-based alloy is a nanoparticle with a hollow structure, the modified graphene is an oleophobic modified graphene, and the solvent is either ethanol or acetone; The modified graphene can be prepared by a covalent bonding method, and the particle size of the modified graphene is 50nm to 300nm; The mass fraction of each element in the nickel-based alloy is: C: 0.7% to 1.1%, B: 3.0% to 4.0%, Si: 3.5% to 5.0%, Cr: 17.0% to 20.0%, Cu: 0 to 0.5%, Fe: 0 to 5%, Mo: 2.0% to 3.0%, rare earth: 2.0% to 3.0%, and the balance is Ni and unavoidable impurities; The preparation method of the high-strength anti-corrosion coating for oil casing is as follows: Step A, preparing the nickel-based alloy into nanoparticles: crushing and grinding the nickel-based alloy, placing the alloy powder in a high-temperature furnace, and forming nano-scale nickel-based alloy particles at 800° C.-1000° C. by chemical vapor deposition or physical vapor deposition; Step B, forming a hollow structure of the nickel-based alloy: placing the nano-scale nickel-based alloy prepared in step A in a specific template, immersing the template and the nickel-based alloy in an acidic or alkaline solution, the ions in the solution react with the surface of the template to form holes on the surface of the template, and sintering the nickel-based alloy with holes at a high temperature to solidify the nickel-based alloy and form a hollow structure; Specifically, the specific template is polystyrene microspheres, the reaction time between the template and the nickel-based alloy nanoparticles is 6-10 hours, the sintering temperature of the high-temperature sintering is 800°C-1200°C, and the sintering time is 9-16 hours; Step C, filling modified graphene: modifying the graphene, and filling the modified graphene into the hollow structure of the nickel-based alloy through surface modification treatment to obtain an anti-corrosion coating; The modification and filling methods of graphene are specifically as follows: Step C-1, functionalizing the graphene to introduce functional groups suitable for covalent bonding, wherein the functionalization method is either reduction of graphene oxide or conversion of functional groups on the graphene oxide; Step C-2, introducing an activation group on the functionalized graphene surface, reacting the molecule containing the oleophobic group with the activated graphene surface to form a covalent connection; Step C-3, purifying and characterizing the covalently linked graphene to ensure that the oleophobic groups are successfully linked to the graphene surface; Step C-4, adding the modified graphene powder into a solvent, and adding an appropriate amount of a surfactant, dispersing the graphene in the solution by ultrasonic treatment or stirring to prepare a uniform graphene dispersion; Step C-5, pouring the prepared graphene dispersion into the nickel-based alloy with a hollow structure, ensuring that the material is completely covered and impregnated, and performing an impregnation treatment so that the graphene fully penetrates into the nickel-based alloy with a hollow structure; Step D, coating: coating the prepared anti-corrosion coating on the surface of the oil casing, drying the coated coating, and then curing the coating to firmly bond the coating to the metal substrate.
2. The method for preparing a high-strength anti-corrosion coating for oil casing according to claim 1, Features: In step C-5, the sample after immersion is dried to remove the residual solvent by natural air drying or heating drying.
Citation Information
Patent Citations
Anticorrosive nanopaint prepared from graphene, superconducting elements and rare earth elements