Environmentally friendly multifunctional leavening agent and preparation method thereof

By using environmentally friendly multifunctional leavening agents combined with amide solvents and surfactants, the problem of insufficient leavening of the traditional leavening agents on the slag is solved, the yield of PCB boards is improved and the environmental protection and wastewater treatment costs are reduced. .

CN118599602BActive Publication Date: 2024-12-03HUI ZHOU WING ON DA CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410640081.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2024-12-03
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

Traditional leavening agents have low looseness to the slag, resulting in low yield of PCB boards, and have great requirements for environmental pollution and wastewater treatment, which has environmental protection problems.

Method used

Using amide solvents, polyethylene glycol diglycidyl ether and isopropanolamine as permeability system, combined with surfactant, dispersant and tackifier, an environmentally friendly multifunctional leavening agent can effectively penetrate into the gum The inside of the slag is softened and evenly dispersed, improving the expansion efficiency, and does not contain organic solvents and strong alkalis, making it easy to treat wastewater.

Benefits of technology

It significantly improves the softening and loosening effect of the leavening agent on the glue slag, improves the surface hydrophilicity and uniformity of the PCB base resin, improves the efficiency and yield of the subsequent glue slag removal process, and has good environmental protection. , reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present application relates to the field of circuit board processing technology, and specifically discloses an environmentally friendly multifunctional leavening agent and a preparation method thereof. An environmentally friendly multifunctional leavening agent is prepared from the following raw materials in weight percentage: 45-55% amide solvent, 12-18% polyethylene glycol diglycidyl ether, 5-10% isopropanolamine, 3-8% dispersant, 4-6% tackifier, 2-5% surfactant and residual water; preparation method: dispersant, surfactant and water are mixed; amide solvent, polyethylene glycol diglycidyl ether and oleic acid amide propyl dimethyl tertiary amine are added to mix; tackifier is added to heat and mix. The leavening agent of the present application has good environmental protection and uniform permeability, can fluff and soften the glue residue in the borehole, is conducive to the later desmearing agent to bite the glue residue in the borehole, and forms a uniform honeycomb morphology on the surface of the borehole wall, which is conducive to the later copper deposition, and the obtained PCB board has a high backlight level and a high yield rate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of circuit board processing technology, and more specifically, to an environmentally friendly multifunctional leavening agent and a preparation method thereof. Background Art

[0002] The process flow of PCB horizontal copper deposition is: bulking - desmearing - pre-neutralization - neutralization - hole filling - micro-etching - pre-impregnation - activation - reduction - copper deposition. It has a high degree of automation, short process time, sealed production line, and is easy to carry out 5S management. It is the preferred PCB manufacturing process for various circuit board factories.

[0003] Among them, the effect of the expander as the first step of horizontal copper deposition of PCB is the key to quality assurance in the PCB manufacturing process. This is because when drilling, the PCB substrate resin will rise to a higher temperature during the high-speed rotation and intense friction of the drill bit. When the temperature exceeds the Tg temperature of the PCB substrate resin, the PCB substrate resin will be melted into a paste and coated on the hole wall. After cooling, it becomes glue residue. If the expander step is not performed before removing the glue residue, it will cause the drilling contamination in the hole to be not completely removed or over-etching.

[0004] At present, the commonly used leavening agents are solvents such as acetone and toluene or strong alkaline leavening agents. In actual application, these leavening agents have weak ability to make the glue residue fluffy, and the yield rate of the produced PCB boards is low. At the same time, traditional leavening agents have high requirements for wastewater discharge and treatment, which easily cause environmental pollution and wastewater treatment costs. Summary of the invention

[0005] In order to solve the problem that traditional leavening agents have low leavening properties for slag, thereby reducing the yield of the produced PCB boards, the present application provides an environmentally friendly multifunctional leavening agent and a preparation method thereof.

[0006] In the first aspect, the present application provides an environmentally friendly multifunctional leavening agent, which adopts the following technical solution:

[0007] An environmentally friendly multifunctional leavening agent is prepared from the following raw materials in percentage by weight:

[0008] Amide solvent 45-55%

[0009] Polyethylene glycol diglycidyl ether 10-18%

[0010] Isopropanolamine 5-10%

[0011] Dispersant 3-8%

[0012] Tackifier 4-6%

[0013] Surfactant 2-5%

[0014] Water balance.

[0015] By adopting the above technical scheme, amide solvents, polyethylene glycol diglycidyl ether and isopropanolamine are used as the penetration system, which can penetrate into the interior of the glue residue, have a good swelling effect on the glue residue, reduce the bond energy between the glue residue molecules, and soften the glue residue in the drilled hole of the PCB substrate resin. The surfactant can reduce the surface tension of the surface of the PCB substrate resin, so that the prepared swelling agent can quickly penetrate into the drilled hole, and the softening efficiency of the glue residue is improved. The dispersant and the viscosity enhancer can have a good uniform dispersion effect on the swelling agent, so that the swelling agent can be evenly dispersed and attached to the hole wall of the drilled hole, and the glue residue is adsorbed and softened. The softening and bulking efficiency of the glue residue is improved in one step; the bulking agent prepared in the present application has a good softening and bulking effect on the glue residue, is easy to carry out the subsequent desmearing process, improves the hydrophilicity and uniformity of the surface of the PCB substrate resin, can promote the subsequent desmearing agent to uniformly bite the hole wall of the PCB substrate resin, form a uniformly distributed honeycomb morphology, improve the adhesion and uniformity of the subsequent copper plating treatment, and then improve the yield of the prepared PCB board; the bulking agent of the present application does not add organic solvents such as toluene and acetone, nor does it add substances such as strong alkali, has good environmental protection, is easy to be removed for wastewater treatment, and saves production costs.

[0016] Preferably, the amide solvent is one or a combination of N,N-dimethylformamide, N,N-dimethylacetamide, and N-trimethylsilylacetamide.

[0017] By adopting the above technical solution, the above amide solvent has good permeability and swelling property, and can quickly penetrate into the glue residue to soften the glue residue.

[0018] Preferably, the dispersant is one or a combination of sodium citrate, sodium sulfate, sodium acetate, sodium gluconate, and sodium thiosulfate.

[0019] By adopting the above technical solution, the above dispersant has good dispersing performance and can further improve the dispersing permeability of the leavening agent to the rubber residue.

[0020] Preferably, the dispersant consists of sodium gluconate and sodium thiosulfate in a weight ratio of (2-4):1.

[0021] By adopting the above technical solution and using sodium gluconate and sodium thiosulfate in a better ratio as dispersants, the penetration uniformity of the leavening agent inside the drilled holes on the surface of the PCB substrate resin can be improved, and the softening and leavening efficiency of the glue residue can be further improved.

[0022] Preferably, the surfactant is composed of sodium fatty alcohol polyoxyethylene ether carboxylate and dodecyl dimethyl amine oxide in a weight ratio of (1-2):1.

[0023] By adopting the above technical scheme, the surfactant with the optimal dosage ratio has good hydrophilicity and good charge adsorption effect, which can further improve the affinity between the leavening agent and the PCB substrate resin, increase the contact area, and further improve the softening and leavening efficiency of the leavening agent on the slag. At the same time, it is beneficial for the later slag removal agent to bite the drill hole wall of the PCB substrate resin and improve the uniformity of the bite.

[0024] Preferably, the viscosity enhancer is one or a combination of hydroxyethyl cellulose, starch, magnesium aluminum silicate, kaolin, hydroxypropyl guar gum, and oleamidopropyl dimethyl tertiary amine.

[0025] By adopting the above technical solution, the above-mentioned viscosity enhancer has good viscosity, and the leavening agent prepared therefrom has good adhesion, which can improve the adhesion performance of the leavening agent on the surface of the rubber residue, and further improve the leavening and softening efficiency of the leavening agent on the rubber residue.

[0026] Preferably, the viscosity enhancer is composed of hydroxypropyl guar gum, magnesium aluminum silicate and oleamidopropyl dimethyl tertiary amine in a weight ratio of 1:(1-3):(1-2).

[0027] By adopting the above technical scheme, hydroxypropyl guar gum, magnesium aluminum silicate and oleic acid amide propyl dimethyl tertiary amine in a relatively optimal ratio are used as thickeners, which can produce a good synergistic effect with amide solvents, polyethylene glycol diglycidyl ether and isopropanolamine. The prepared leavening agent has good adhesion stability, further improves the uniformity and stability of the leavening agent's penetration of glue residue, further improves the leavening and softening effects on the glue residue, is beneficial to the uniform biting of the drill hole wall by the later desmear agent, and improves the finished product yield of the prepared PCB board.

[0028] Preferably, the viscosity of the environmentally friendly multifunctional leavening agent is 60-150 mPa·s.

[0029] By adopting the above technical solution, the leavening agent with better viscosity has better adhesion and better permeability.

[0030] In a second aspect, the present application provides a method for preparing an environmentally friendly multifunctional leavening agent, which adopts the following technical scheme: A method for preparing an environmentally friendly multifunctional leavening agent, comprising the following preparation steps:

[0031] S1. Add a dispersant and a surfactant into water, stir and dissolve, and prepare a mixture A;

[0032] S2. Add amide solvent, polyethylene glycol diglycidyl ether and oleic acid amide propyl dimethyl tertiary amine to mixture A, mix well, add thickener, heat and stir well to obtain an environmentally friendly multifunctional leavening agent.

[0033] By adopting the above technical scheme, the dispersant and the surfactant are first dissolved in water, then the amide solvent, polyethylene glycol diglycidyl ether and oleic acid amide propyl dimethyl tertiary amine are added, and finally the viscosity of the system is adjusted by adding a thickener. The leavening agent prepared in this way has good system stability and viscosity.

[0034] Preferably, the heating and stirring temperature in step S2 is 40-50°C.

[0035] By adopting the above technical solution, the optimal heating and stirring temperature can make the thickener dissolve evenly and improve the dissolution efficiency.

[0036] In summary, this application has the following beneficial effects:

[0037] 1. The environmentally friendly multifunctional leavening agent of the present application uses amide solvents, polyethylene glycol diglycidyl ether and isopropanolamine as the penetration system, and then compounded with a dispersant, a surfactant and a tackifier. The four produce a good synergistic effect. The prepared leavening agent has a good softening and leavening effect on the glue residue, which is easy to carry out the subsequent desmearing process, improves the hydrophilicity and uniformity of the surface of the PCB substrate resin, and can promote the subsequent desmearing agent to uniformly bite the hole wall of the PCB substrate resin to form a uniformly distributed honeycomb morphology, improve the adhesion and uniformity of the subsequent copper plating treatment, and thus improve the yield of the prepared PCB board; the leavening agent of the present application does not add organic solvents such as toluene and acetone, nor does it add substances such as strong alkali, has good environmental protection, is easy to remove wastewater treatment, and saves production costs.

[0038] 2. By using a better ratio of sodium gluconate and sodium thiosulfate as dispersants, hydroxypropyl guar gum, magnesium aluminum silicate and oleic acid amide propyl dimethyl tertiary amine as thickeners, it can produce a good synergistic effect with amide solvents, polyethylene glycol diglycidyl ether and isopropanolamine. The prepared leavening agent has good dispersion uniformity and adhesion stability, further improving the uniformity and stability of the leavening agent's penetration of the glue residue, and further improving the bulking and softening effect of the glue residue, which is beneficial to the uniform bite of the later desmear agent on the drill hole wall, and improving the finished product yield of the prepared PCB board.

[0039] 3. The preparation method of the present application is simple, and an environmentally friendly multifunctional leavening agent with stable performance, good softening and leavening effects on rubber residue is obtained. DETAILED DESCRIPTION

[0040] The present application is further described in detail below with reference to the embodiments.

[0041] The following are the sources and specifications of some raw materials for this application:

[0042] 1. Polyethylene glycol diglycidyl ether: CAS No. 39443-66-8;

[0043] 2. Oleic acid amidopropyl dimethyl tertiary amine: CAS No. 109-28-4, content 98%;

[0044] 3. Sodium fatty alcohol polyoxyethylene ether carboxylate: solid content 28±1%, 10% aqueous solution pH = 11.5-12.5;

[0045] 4. Hydroxyethyl cellulose: Dow, QP 4400H;

[0046] 5. Starch: corn starch, CAS No. 9005-25-8;

[0047] 6. Magnesium aluminum silicate: 1250 mesh, content 99%, CAS number 71205-22-6;

[0048] 7. Kaolin: 1250 mesh, silica content 50-70%;

[0049] 8. Hydroxypropyl guar gum: gm, content 98%.

[0050] Example

[0051] Example 1

[0052] Example 1 discloses an environmentally friendly multifunctional leavening agent, which is prepared by the following steps:

[0053] S1, add 2kg of sodium citrate and 1kg of sodium sulfate as dispersants and 3kg of sodium dodecylbenzene sulfonate and 2kg of sodium fatty alcohol polyoxyethylene ether sulfate as surfactants into 15kg of water, stir for 20min, stir and dissolve to obtain a mixture A;

[0054] S2. Add 45 kg of N,N-dimethylformamide as an amide solvent, 18 kg of polyethylene glycol diglycidyl ether and 10 kg of isopropanolamine to mixture A, mix for 10 minutes, and after mixing evenly, add 2 kg of hydroxyethyl cellulose and 2 kg of hydroxypropyl guar gum as thickeners, heat to 40°C, stir for 1 hour, and stir evenly to obtain an environmentally friendly multifunctional leavening agent.

[0055] Example 2-3

[0056] The difference between Example 2-3 and Example 1 is that the amount of raw materials used and the preparation conditions are different, see Table 1 below for details.

[0057] Table 1 Raw material dosage and preparation conditions of Examples 1-3

[0058]

[0059]

[0060] Example 4

[0061] The difference between Example 4 and Example 3 is that the dispersant is different. The dispersant in Example 4 consists of sodium gluconate and sodium thiosulfate. The amount of sodium gluconate is 5.33 kg, and the amount of sodium thiosulfate is 2.67 kg. The rest is the same as Example 3.

[0062] Example 5

[0063] The difference between Example 5 and Example 4 is that the amount of sodium gluconate is 6.4 kg, the amount of sodium thiosulfate is 1.6 kg, and the others are the same as Example 3.

[0064] Example 6

[0065] The difference between Example 6 and Example 4 is that the surfactant is different. The surfactant in Example 6 is composed of sodium fatty alcohol polyoxyethylene ether carboxylate and dodecyl dimethyl amine oxide. The amount of sodium fatty alcohol polyoxyethylene ether carboxylate is 1 kg, and the amount of dodecyl dimethyl amine oxide is 1 kg. The rest is the same as Example 4.

[0066] Example 7

[0067] The difference between Example 7 and Example 6 is that the amount of sodium fatty alcohol polyoxyethylene ether carboxylate used is 1.33 kg, the amount of dodecyl dimethyl amine oxide used is 0.67 kg, and the rest is the same as Example 6.

[0068] Example 8

[0069] The difference between Example 8 and Example 6 is that the thickener is different. The thickener in Example 8 is composed of hydroxypropyl guar gum, magnesium aluminum silicate and oleamidopropyl dimethyl tertiary amine. The amount of hydroxypropyl guar gum is 1.25 kg, the amount of magnesium aluminum silicate is 1.25 kg, and the amount of oleamidopropyl dimethyl tertiary amine is 2.5 kg. The rest is the same as Example 6.

[0070] Example 9

[0071] The difference between Example 9 and Example 8 is that the amount of hydroxypropyl guar gum used is 1 kg, the amount of magnesium aluminum silicate used is 3 kg, the amount of oleamidopropyl dimethyl tertiary amine used is 1 kg, and the rest is the same as Example 8.

[0072] Comparative Example

[0073] Comparative Example 1

[0074] The difference between Comparative Example 1 and Example 3 is that an equal amount of isopropanolamine is replaced by N,N-dimethylformamide, and the rest is the same as Example 3.

[0075] Comparative Example 2

[0076] The difference between Comparative Example 2 and Example 3 is that an equal amount of polyethylene glycol diglycidyl ether is replaced by isopropanolamine, and the rest is the same as Example 3.

[0077] Comparative Example 3

[0078] The difference between Comparative Example 3 and Example 3 is that the viscosity enhancer is replaced by a dispersant in equal amount, and the rest is the same as Example 3.

[0079] Performance testing

[0080] The following is a performance test of the environmentally friendly multifunctional leavening agents prepared in Examples 1-9 and Comparative Examples 1-3:

[0081] 1. Test on the corrosion resistance of PCB substrate resin

[0082] A 1mm thick epoxy resin PCB substrate with holes was first bulked with a bulking agent and then desmeared to test the bite amount (unit: mg / dm 2 ), and observe the uniformity of the honeycomb morphology of the PCB substrate after the bite in the SEM electron microscope. The uniformity of the honeycomb surface morphology is evaluated using the following grades:

[0083] If the uneven area accounts for less than 5%, it is recorded as level 1;

[0084] The uneven area accounts for 6-10%, which is recorded as level 2;

[0085] The uneven area accounts for 11-15%, which is recorded as level 3;

[0086] The uneven area accounts for 16-20%, which is recorded as level 4;

[0087] If the uneven area accounts for more than 20%, it is recorded as level 5;

[0088] The parameters of bulking treatment are as follows:

[0089] Soaking in leavening agent solution at 70°C for 6 minutes;

[0090] The desmear treatment parameters are as follows: immersion treatment with desmear agent stock solution, temperature 75° C., time 13 min; the desmear agent is prepared from the following raw materials in weight percentage: 5.5% potassium permanganate, 5.5% sodium hydroxide and 89% water.

[0091] 2. PCB board backlight level test:

[0092] A 1mm thick epoxy resin PCB substrate board with holes drilled was subjected to a process of swelling-slag removal-pre-neutralization-neutralization-hole filling-micro-etching-pre-impregnation-activation-reduction-horizontal chemical copper to obtain a PCB board, and then the backlight level of the PCB board was measured; wherein, the pre-neutralization and neutralization treatments were both performed using a 5wt% sulfuric acid aqueous solution at a temperature of 40°C for 50s;

[0093] The pore-forming treatment uses a pore-forming agent soaking treatment, and the soaking agent is made of the following raw materials in weight percentage: 10% diethylenetriamine, 2% imidazoline and 88% water; the temperature is 50° C., and the time is 60 seconds;

[0094] The micro-etching treatment uses a micro-etching agent immersion treatment, and the micro-etching agent is made of the following raw materials in weight percentage: 3% sulfuric acid, 6% sodium persulfate and 91% water, the temperature is 30°C, and the time is 30s;

[0095] The pre-preg treatment used a 10 wt % sodium carbonate aqueous solution at 30 ° C for 30 s;

[0096] The activation treatment uses an activator soaking treatment, the activator is made of the following raw materials in weight percentage: 0.05% palladium sulfate, 2% sodium carbonate, 2% triethylamine, 1% fatty alcohol polyoxyethylene ether and 94.95% water, the temperature is 50°C, and the time is 45s;

[0097] The reduction treatment used a 10 wt % boric acid aqueous solution at 30 ° C for 35 s;

[0098] Horizontal chemical copper uses horizontal chemical copper deposition agent, including liquid A, liquid B and formaldehyde. Liquid A is prepared from the following raw materials in weight percentage: 5% copper sulfate, 1% potassium sodium tartrate, 0.2% thiourea and 93.8% water. Liquid B is prepared from the following raw materials in weight percentage: 14% sodium hydroxide, 2% sodium dihydrogen phosphate and 84% water. When used, 50g / L of liquid A, 50g / L of liquid B, 70g / L of formaldehyde, and the balance of water are used at a temperature of 38°C and a time of 360s.

[0099] The following are the performance test data of the environmentally friendly multifunctional leavening agents prepared in Examples 1-9 and Comparative Examples 1-3, see the table below for details.

[0100] Table 2 Performance test data of environmentally friendly multifunctional leavening agents prepared in Examples 1-9 and Comparative Examples 1-3

[0101]

[0102] It can be seen from Examples 1-3 and 4-5 and Table 2 that the use of a dispersant in an optimal proportion of the present application can improve the dispersibility of the leavening agent on the glue residue, increase the amount of bite of the glue residue, improve the uniformity of the honeycomb morphology on the surface of the PCB substrate resin, and improve the backlight level of the prepared PCB board, with a high yield of the finished product.

[0103] Combining Examples 4-7 and Examples 8-9, Comparative Example 3 and Table 2, it can be seen that the use of a preferred ratio of the viscosity enhancer in the present application plays a greater role in improving the performance of the leavening agent, and the amount of bite of the rubber residue can reach 69 mg / dm 2 A uniform honeycomb morphology is formed on the surface of the PCB substrate resin, and the backlight level of the prepared PCB board also reaches level 10; in Comparative Example 3, the tackifier is replaced by a dispersant, and the performance of the leavening agent is significantly reduced, indicating that the use of the dispersant and the tackifier of the present application to cooperate has a greater effect on improving the performance of the leavening agent.

[0104] It can be seen from Examples 1-3 and Comparative Examples 1-2 and Table 2 that the use of the amide solvent, polyethylene glycol diglycidyl ether and isopropanolamine compound of the present application has a good softening and swelling effect on the glue residue, which is beneficial to the subsequent degumming agent to uniformly bite the PCB substrate resin, and the obtained PCB board has a high backlight level; the performance of the swelling agent prepared in Comparative Examples 1-2 is significantly reduced.

[0105] The environmentally friendly multifunctional leavening agent prepared in the present application has a viscosity of 60-150 mPa·s / 25°C, has good adhesion and penetration stability, can evenly soften and leaven the glue residue, and is conducive to the later desmear agent to evenly bite the drilling hole wall of the PCB substrate resin, thereby improving the finished product yield of the PCB board.

[0106] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An environmentally friendly multifunctional leavening agent, characterized in that: Made from the following raw materials in weight percentage: Amide solvent 45-55% Polyethylene glycol diglycidyl ether 10-18% Isopropanolamine 5-10% Dispersant 3-8% Thickener 4-6% Surfactant 2-5% Water balance; The dispersant is composed of sodium gluconate and sodium thiosulfate in a weight ratio of (2-4):1; The surfactant is composed of sodium fatty alcohol polyoxyethylene ether carboxylate and dodecyl dimethyl amine oxide in a weight ratio of (1-2):1; The viscosity enhancer is composed of hydroxypropyl guar gum, magnesium aluminum silicate and oleamidopropyl dimethyl tertiary amine in a weight ratio of 1:(1-3):(1-2).

2. An environmentally friendly multifunctional leavening agent according to claim 1, characterized in that: The amide solvent is one or a combination of N,N-dimethylformamide, N,N-dimethylacetamide and N-trimethylsilylacetamide.

3. An environmentally friendly multifunctional leavening agent according to claim 1 or 2, characterized in that: The viscosity of the environmentally friendly multifunctional leavening agent is 60-150 mPa•s.

4. A method for preparing an environmentally friendly multifunctional leavening agent as claimed in any one of claims 1 to 3, characterized in that: The method comprises the following preparation steps: S1. Add a dispersant and a surfactant into water, stir and dissolve, and prepare a mixture A; S2. Add amide solvent, polyethylene glycol diglycidyl ether and isopropanolamine to mixture A, mix well, add tackifier, heat and stir well to obtain an environmentally friendly multifunctional leavening agent.

5. The method for preparing an environmentally friendly multifunctional leavening agent according to claim 4, characterized in that: The heating and stirring temperature in step S2 is 40-50°C.